Alternate Names: Pyrophillite
Description: A Soft Hydrous Aluminum Silicate
Formula: Al2O3.4SiO2.H2O
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| Al2O3 | 28.30% | 1.00 | |
| SiO2 | 67.70% | 4.06 | |
| LOI | 4.00% | n/a | |
| Oxide Weight | 346.01 | ||
| Formula Weight | 360.42 | ||
Pyrophyllite is a low-expansion mineral. The individual particles expand less on heating (and therefore contract less on cooling) than other refractory particles (like silica). Thus, during firing, pyrophyllite particles counter the shrinkage of the plastic components surrounding them (assuming that particles remain whole and undissolved to exert their influence on the surrounding matrix). Pyrophyllite-refractory clay combinations potentially have excellent volume stability and resistance to deformation at high temperatures. Pyrophyllite has a second expansion-lowering mechanism: Its presence in stoneware and porcelain bodies can encourage the development of more mullite, which both increases firing strength and reduces thermal expansion. In this case, the individual particles of pyrophyllite react and transform from their original state.
In clay bodies, substitution of part or all of the silica will decrease thermal expansion (see also kyanite, mullite) while maintaining the level of maturity (although some adjustment in the feldspar will likely be needed). However, this will of course mean that glazes may need to be adjusted (or they will craze). Oftentimes, glaze fit takes priority, and it is actually better to leave the silica content at 20-25% (silica increases thermal expansion and improves glaze fit).
In glazes, Pyrophyllite is a better source of SiO2 than quartz (if its iron content can be tolerated). This is because the latter is slow to dissolve into the melt, often much is left undissolved (affecting the transparency). Also, since the SiO2 become an integral part of the glass, its theoretical expansion-lowering effect is more fully realized.
When substituted for feldspar, pyrophyllite will decrease body maturity, firing shrinkage and thermal expansion. Strength may also be increased (even though the body is less vitreous).
In electrical porcelain, large amounts (up to 95%) may be used in bodies for optimal electrical properties and high frequency characteristics (where zero porosity is not critical).
Pyrophyllite is also used as an ingredient in wall tile bodies since it has the effect of reducing moisture expansion.
Because of its stable nature and physical properties, pyrophyllite is employed in mold release and parting agents in foundry and structural clay products.
Pyrophyllite is ideal for certain types of refractories because no calcining is needed. Its physical nature also helps to reduce wear and tear on molds and machinery that handle wet and dry product.
Some grades of pyrophyllite have a higher iron content and can darken the color of porcelain bodies. For sanitary ware bodies where the translucency and fired color are not important, pyrophyllite can be added to reduce pyroplastic deformation (especially where talc is employed as an auxiliary flux).
Also, porcelains that are highly vitreous (from high feldspar or frit content) can take pyrophyllite particles into solution; when this happens the effect of their low expansion properties is lost on the body.
Pyrax (Pyrophillite) is a mineral having a very low thermal expansion. It stands to reason that if we can maximize its percentage in a body and not fire the body to a point that changes the crystal structure, it will be resistant to thermal-shock cracking. To that end, I mixed it with only kaolin (ball clay would add some quartz that would increase thermal expansion). I made slip-cast pieces of similar thickness for testing. I fired them to cone 2 (after finding that by cone 4, shock-resistance begins to decline). As you can see from the video, the addition of grog actually harms the performance! The higher the Pyrax, the better. To get a real appreciation for how well this body endures differential heat stress, wait till the end to see how a glazed porcelain piece compares.
| URLs |
http://en.wikipedia.org/wiki/Pyrophyllite
Pyrophyllite at Wikipedia |
| Minerals |
Pyrophyllite
Pyrophyllite is an aluminum silicate mineral with a similar chemical structure to talc (a magnesium |
| Typecodes |
Refractory
Materials that melt at high temperatures. These are normally used for kiln bricks, furniture, etc. or for ceramics that must withstand high temperatures during service. |
| Typecodes |
Low Expansion Material
Materials used to make bodies requiring low expansion (e.g. flameware, refractories). The individual particles of these materials have low expansion. Some of theme even expand at certain temperature ranges. |
| Typecodes |
Aluminum Silicate
Materials not classifiable as commonly known aluminum silicates. For example, kaolin is a common aluminum silicate. |
| Typecodes |
Generic Material
Generic materials are those with no brand name. Normally they are theoretical, the chemistry portrays what a specimen would be if it had no contamination. Generic materials are helpful in educational situations where students need to study material theory (later they graduate to dealing with real world materials). They are also helpful where the chemistry of an actual material is not known. Often the accuracy of calculations is sufficient using generic materials. |
| Materials |
Pyrax HS
|
| Materials |
Pyrax RG
|
| Materials |
Pyrax Pyrophyllite
|
| Materials |
Sericite Y/T
A commercial grade of sericite mineral. |
| Materials |
Kyanite
A refractory aluminum silicate mineral notable for low thermal expansion and one-way volume expansion as it converts to mullite at high temperatures. |
| Materials |
Pyrofrac
|
| Materials |
Pyrophyl
|
| Materials |
Pyrofrac 2023
|
| Materials |
Pyrofrac 1855
|
| Materials |
Pyrofrac 1655
|
| Materials |
Pyrofrac 1004
|
| Materials |
Pyrofrac 0304
|
| Materials |
Pyrofrac 0204
|
| Materials |
Andalusite
A low expansion aluminum silicate mineral that converts to mullite on repeated firings. |
| Materials |
Mullite
A highly refractory low-expansion alumino-silicate crystal formed naturally only rarely but produced industrially and within fired kaolin bodies. |
| Materials |
Pyrofrac 2024
|
| Materials |
Pyrofrac 2034
|
| Materials |
Pyrophyl R-1403
|
| Materials |
Pyrophyl R-2252
|
| Materials |
Pyrophyl R-2253
|
| Materials |
Alkatrol
|
| Materials |
Talc
A source of MgO for ceramic glazes, a flux or thermal expansion additive in clay bodies, also used in the manufacture of cordierite. |
| Materials |
Virginia Kyanite
|
| Materials |
Pyrofrac 4205
|
| Materials |
Pyrofrac 4203
|
| Body Thermal Expansion | Pyrophyllite is often included in bodies to reduce thermal expansion. |
|---|