Alternate Names: Disthene, Cyanite
Formula: Al2O3.SiO2
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| Al2O3 | 62.92% | 1.00 | |
| SiO2 | 37.08% | 1.00 | |
| Oxide Weight | 162.11 | ||
| Formula Weight | 162.11 | ||
Kyanite is a refractory material, normally used in granular form (or granular/powder mix). The grains have relatively low thermal expansion so their presence in a material imparts resistance to thermal shock. Kyanite is widely employed in insulating brick, kiln furniture, refractory shapes, crucibles, etc. and in porcelain, tile bodies, and casting mixes. The material reduces fired shrinkage, increases mechanical strength and thermal shock resistance and allows products to be made with thinner walls, better resistance to dunting, deformation and chipping. Two keys to its usefulness are its refractory character and that it expands as it converts to mullite (while almost all ceramic materials shrink as they fire).
Kyanite has properties that make it very different from most ceramic raw materials:
-Starting around 1100C, kyanite begins to decompose to form mullite crystals (making it a convenient mullite precursor in many refractory compositions). This conversion can occur in a single high-temperature firing or progressively over multiple firings at lower temperatures. Some industrial applications deliberately calcine kyanite first to complete this transformation before use.
-Kyanite grains expand significantly during this conversion (typically about 4–8%, depending on particle size, firing temperature, soak time). This unusual irreversible expansion is valuable in refractory and thermal-shock-resistant applications because it can offset normal body shrinkage.
-Its particles resist sintering together during firing. Because expansion tends to separate particles rather than pull them into contact, kyanite does not readily develop self-bonding strength. For this reason, other materials must supply the bonding phase: kaolin is commonly used in lower-temperature systems, while mullite-forming clays, alumina, or other refractory binders are preferred at higher temperatures.
Among the Al₂SiO₅ minerals (polymorphs kyanite, andalusite, sillimanite), kyanite produces the greatest volume increase because its crystal structure undergoes the largest rearrangement. This can make it less preferred in some applications because it creates more firing stress, conversion is less controlled and dimensional stability is harder to predict. Kyanite can also generate internal stresses if coarse particles are used in thick sections because some grains convert before others.
Kyanite’s elongated, angular particles contribute additional advantages in ceramic bodies. They tend to interlock mechanically, creating a crystal framework that helps resist shrinkage even in bodies fired to relatively low temperatures. This is why potters often use it in thermal-shock-resistant bodies such as raku, sometimes at additions up to 30%.
Coarse kyanite (e.g. 35–48 mesh) is often preferred when the goal is thermal shock resistance. Particles act like miniature aggregate, interrupting crack propagation and particle-by-particle expansion helps offset body shrinkage. In addition, the elongated grains interlock mechanically and the more open structure improves resistance to thermal gradients. That is why coarse kyanite is common in raku bodies, kiln furniture, burner blocks and refractory castables. Because of its particle geometry, surprisingly high percentages of coarse kyanite can be added without severely reducing workability in smooth plastic throwing bodies. Additions of 10–15% such as 48 mesh, for example, can increase green strength, improve drying behavior, and reduce drying shrinkage while still preserving acceptable plasticity and maintaining a relatively smooth feel.
Fine kyanite behaves much more uniformly and conversion to mullite begins sooner (because surface area is greater). In addition, expansion is distributed more evenly. Fine grades are useful in fine refractories, engobes, smoother stoneware bodies and precision refractories.
Kyanite is available in grain sizes down to 325 mesh. Because the long thin crystals irreversibly expand and interlock on initial heatup, they hold the material tightly into place. The density is enhanced further when granule/powder forms of the material are used. This expansion phenomenon has proven invaluable in cements, crack fillers, ramming mixes, and mortars. And even in stoneware bodies to counteract the shrinkage during firing.
Kyanite is found in large deposits in India, Africa and the USA. American kyanite occurs in association with quartz, from which it must be mechanically separated by grinding. Indian kyanite is processed from surface boulders and can be calcined in lump form and graded in coarser sizes. American kyanite is said to be the most consistent and Indian the purest.

This picture has its own page with more detail, click here to see it.
Plainsman M390 with 12.5% 48 mesh kyanite wedged in. This was added to improve the drying properties while maintaining the plasticity. However, the throwing also improved! It was easier to pull up into a tall cylinder. The surface texture is only moderately disrupted by a slight graininess.

This picture has its own page with more detail, click here to see it.
Plainsman M340 with 11% added 48 mesh kyanite. The kyanite was added to improve the plastic strength to stand up when throwing large shapes. It has done this. Its grainy texture (in an otherwise smooth body) is only slightly noticeable while throwing, but it lifts better. The kyanite was simply wedged into the clay using a slice-and-wedge technique, the stiffness was affected only slightly. An added benefit will be a reduction in the thermal expansion (and thus thermal utility) of the fired clay (of course there is a chance that glazes will need to be adjusted to deal with crazing).

This picture has its own page with more detail, click here to see it.
The goblet on the left is bending, not just because the clay is somewhat unstable at the temperature being fired, but because this shape is also inherently unstable. Where extreme shapes are prone to warping, ware must be made from clays that do not vitrify (that introduces issues of strength and functionality). In this case, the clay recipe is based on a terra cotta material that matures at a very low temperature. The problem was dealt with by employing a recipe of 60:40 clay:200# kyanite.

This picture has its own page with more detail, click here to see it.
Samples fired to cone 6. Lower left: Plainsman M390. Upper left: M390 plus 12.5% 48 mesh kyanite (no visible effect on fired color or character). Upper right: M390 plus 12.5% Christie STKO 22S 40 mesh grog (strangely it fires a darker color and appears more vitreous and there is no soluble salts circle). Both grogs were wedged into the clay and did not stiffen it or affect plasticity much (in fact, both were easier to pull up during throwing). The percentage water content went from the 21% to 19% in both.

This picture has its own page with more detail, click here to see it.
Traditional kiln patch or bisque fix products are made by mixing kyanite (with other powders) and sodium silicate. They leverage a special property of kyanite particles: They expand on firing, 5% or more. A 30:70 sodium silicate:kyanite mix shrinks only ~0.5% from wet to dry and ~1% from dry to cone 6. While 48 mesh kyanite has a particle size distribution (from fines to coarse) tuned to maximize density to take advantage of the expansion, that is still amazing.
To test, I tried filling the large gap in a bisque mug handle that was cracked completely in two. The kyanite mixes easily with the sodium silicate to form a cohesive material that can be formed (it hardens on surfaces, even your hands, quickly). Glaze coverage over it is poor, thus commercial products would contain other ingredients to make it more "ceramic" in nature (it should be able to tolerate being mixed with materials used to make porcelains and stonewares, in sufficient concentration its expansion will counter their shrinkage).
| URLs |
http://en.wikipedia.org/wiki/Kyanite
Kyanite at Wikipedia |
| Materials |
Pyrophyllite
A refractory aluminum silicate mineral often used in clay body recipes to lower thermal expansion, control fired maturity, mullite development catalyst, etc. |
| Materials |
Mullite
A highly refractory low-expansion alumino-silicate crystal formed naturally only rarely but produced industrially and within fired kaolin bodies. |
| Materials |
Andalusite
A low expansion aluminum silicate mineral that converts to mullite on repeated firings. |
| Materials |
Sillimanite
A low expansion aluminum silicate mineral that converts to mullite on repeated firings. |
| Materials |
Virginia Kyanite
|
| Typecodes |
Generic Material
Generic materials are those with no brand name. Normally they are theoretical, the chemistry portrays what a specimen would be if it had no contamination. Generic materials are helpful in educational situations where students need to study material theory (later they graduate to dealing with real world materials). They are also helpful where the chemistry of an actual material is not known. Often the accuracy of calculations is sufficient using generic materials. |
| Typecodes |
Refractory
Materials that melt at high temperatures. These are normally used for kiln bricks, furniture, etc. or for ceramics that must withstand high temperatures during service. |
| Typecodes |
Low Expansion Material
Materials used to make bodies requiring low expansion (e.g. flameware, refractories). The individual particles of these materials have low expansion. Some of theme even expand at certain temperature ranges. |
| Temperatures | Kyanite decomposition and volume expansion (1100-1450) |
| Glossary |
Raku
Gas fired rustic ceramic ware is cooled from red-hot in a closed container with organic material. The zero-oxygen atmosphere produced reduces carbonate metal decoration to its metallic form. |
| Frit Softening Point | CONE 37 |
|---|---|
| Density (Specific Gravity) | 3.00 |
| Body Thermal Expansion | Kyanite is a super-duty refractory material with very high resistance to thermal shock (because of the interlocked long thin crystals), it can even be used to make thin lab crucibles which can be heated over a direct flame. |
|---|
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk