44MR | APPO | AVPS | AVSC | BDGC | BDLB | BLOI | BWIW | CCON | CDRY | CEC | CLWC | CMST | COLE | COVB | CSSS | DENS | DFAC | DFDM | DIEL | DNLP | DS | DSHR | DSRN | DSTR | DTMP | EBCT | EM20 | FRFU | FRRD | FRTG | FSHR | FSTR | GBBT | GBMF | GEBR | GLAZ | GLFL | GLHD | GLLE | GSPT | GTTM | HDMI | HEGF | HMA | HMAN | HMOH | IFP | IWCT | L10M | L1M | L20M | L2M | L30M | L5 | L5M | LDW | LOI | LQLM | MDPS | MLRG | MOIP | MOR | MOR5 | MORD | OLAD | P200 | P325 | PBPO | PCE | pHPG | pHPW | PPD | PRSM | PSHP | RC | RHEO | SADR | SAMG | SCLE | SHAB | SIEV | SLBY | SOLU | SPHC | SSAB | SVWT | TGA | THCO | TNST | TREL | TRMN | TSFL | UPSD | WABS | WOPL | WRA | WSR | XREF

GLFL - Glaze Melt Flow - Runway Test

Melt fluidity is very difficult to judge from simple observations on glazed ware or samples. It is also difficult to quantify (since various other factors are involved: e.g. surface tension, entrained bubbles, crystals, unmelted particles). Still, knowing the melt fluidity of a glaze is very important in maintaining consistency, duplicating and understanding it. This test requires a special mold to cast the flow testers.

Note again: This test is done to COMPARE the melt fluidity of glazes (or materials), not to establish an absolute value. It compares the degree and character of two melting materials, showing many subtle and obvious differences. That being said, a tester of standard size, shape and clay composition can equal the playing field enough that absoluteness of the result is possible.

Slurry the powdered glaze or raw material with enough water to make a thick slurry. Blender mix the slurry if needed. Dewater the material on a plaster batt, removing enough water to enable forming several small balls that weigh about 12g. Gummed glazes can be very difficult to dewater; if it is not possible to get a plastic mass, just dry them till crumbly and add enough water back in so that fragments will hold together. Dry the balls. The GBMF test has more information on forming balls from non-plastic materials (glazes containing clays almost always have enough plasticity).

Some materials, such as feldspars, will not melt enough to flow so they need a flux (e.g. we add 15% Ferro Frit 3195 when comparing feldspars at cone 6-10).

Assuming two materials are being compared, choose balls from each that weigh as close to 9g as possible. If needed, use a sharp knife to trim off material to fine-tune the weights. Place the balls in the flow tester. Write the identity (using a ceramic pencil) above the reservoirs of each. Fire the device in the lean-back position to the desired temperature (with a tile below to catch overrun). Take a picture and upload it to your account at insight-live.com.

Flow testing devices: Make your own or buy one from PlainsmanClays.com.
Use a white burning not-too-refractory casting body to make the testers. 50% ball clay, 25 silica, 25 feldspar is a good starting point.

Preparing balls for a melt fluidity test using Veegum


Melt fluidity balls using Veegum

This picture has its own page with more detail, click here to see it.

This method uses 3% Veegum. A 0.01g scale is required (the amount of Veegum needs to be precise since it affects melting). Weigh 11g of the frit and 0.33 of Veegum. Put them in a small ziplock bag, zip it to entrap air and roll the zipper down to inflate it. Shake well to mix. Stir the powder into water (~5-8g) in a small bowl. Pour it onto a plaster slab - it dewaters very quickly (e.g. as little as 10 seconds) - just as the water sheen is gone, peel it up with a rubber rib. Smear it back down and peel it up every few seconds until it is plastic and formable (but not sticky). Roll it into a ball, label it and dry it under a heat lamp (this could take an hour, the Veegum really holds on to the water). When dry we use a sharp knife to cut off enough to bring it down to 9 grams. One caveat: The Veegum is a melting catalyst, balls will flow noticeably more, this is not an issue if you are comparing the melts of two materials (but it is for tests meant to be absolute).

Downloadable 3D model for melt flow tester block mold

Available on the Downloads page


3D rendering of Fusion 360 drawing of glaze melt fluidity tester

This picture has its own page with more detail, click here to see it.

This is a 3D rendering of our melt fluidity tester. We have promoted this device for many years as an effective way to compare fired glaze properties (e.g. melt fluidity, surface tension, bubble retention, crystal growth, transparency, melting range, etc). Open the 3MF file in your slicer, move all pieces off the print bed and unselect them all. Then, print each part by moving it onto the bed and using place-on-face to orient it right. Print the funnel wide-side down with brim. Insert the natch clips and embeds into the holes, pour in the plaster, let it set and finally remove the PLA with a heat gun. You now have a working mold to make slip cast testers. Glue the natches and spacers into the embeds, strap the mold together, glue in the pour spout with slip and finish by filling the mold with slip. If the mold is dry, 10-15 minutes should be enough to get adequate thickness (don't make them too heavy). With 0.8mm thick walls, this drawing 3D prints quickly and is easy to remove when the plaster has set (using a heat gun). The halves interlock using natches (requiring our embeds and related parts). The mold halves can also be lined up by the outer edges before clamping them together (thus not requiring natches).

Testing a new brand of dolomite


Melt fluidity of high dolomite glaze

This picture has its own page with more detail, click here to see it.

Dolomite is a key material for glazes, especially mattes. We were forced to adopt a new brand and needed confidence it was equivalent. Three tests were done to compare the old long-time-use material (IMASCO Sirdar) with a new one (LHoist Dolowhite). The first melt flow tester compares them in a very high dolomite cone 6 recipe formulated for this purpose; the new material runs just slightly more. The second tester is uses the G2934 cone 6 magnesia matte recipe with 5% black stain; the new material runs a little less here. The third test is the high dolomite glaze on a dark burning clay to see the translucency and compare the surface character. They are very close. These three gave us the confidence to proceed.

Glaze melt fluidity comparison:

Same chemistries, different recipes


This picture has its own page with more detail, click here to see it.

At low temperatures, potters want transparents with good clarity to support brilliant colors. Especially on terra cotta bodies. A melt flow test like this enables a comparison one cannot do on using glazed test tiles.

These are two low temperature glazes I use at cone 03, G2931F and G2931K. They have the same chemistry. But F gets its boron from Ulexite, a material with a high LOI (notice how the escaping gases have disrupted the downward flow). The frit-sourced boron version on the right flows cleanly and contains almost no obvious bubbles.

So obviously, one would use the K, right? Not exactly. I used the K version successfully on many pieces. In a thin layer, the ulexite seems to act as its own fining agent, like Gerstley Borate, and the bubbles do merge clear well enough.

Melt fluidity of Albany Slip vs. Alberta Slip at cone 10R


Albany vs Alberta Slip melt

This picture has its own page with more detail, click here to see it.

This is a GLFL test, it employs a slipcast melt flow tester to show the flow patterns of two glazes (or materials), side-by-side. Albany Slip was a pure mined silty clay that, by itself, melted to a glossy dark brown glaze at cone 10R. By itself it was a Tenmoku glaze at high temperatures. Alberta Slip is a recipe of mined clays with added refined minerals that give it a similar chemistry, firing behavior and raw physical appearance. As you can see, the melt fluidity is very similar.

Our G2934Y matte yellow vs. Amaco SM-63 yellow


Amaco SM-63 matte yellow

This picture has its own page with more detail, click here to see it.

Left: Our G2934Y recipe with 12% Cerdec 239416 yellow stain. Right: Amaco SM-63 matte yellow. This GLFL test compares the melt flow of these two in a cone 6 C6DHSC schedule firing. The SM-63 is melting very well and yet is more matte. Its color and character indicate the presence of rutile. Notice its flow has many pinholes, this indicates the presence of materials having significant LOI (these holes are also evident where layer thickness is greater on the tile). The high melt fluidity (indicated by this melt flow tester) is the mechanism behind the way its color intensity varies with the thickness (note the tile on the lower right). The SM-63 also performs well in a cutlery marking test.

Variables

LEN - Length (V)

Suggested units are cm

NOTE - Note (V)

Characterize the flow noting bubbling, blistering, matting, crawling, etc.

Related Information

Links

Articles A Low Cost Tester of Glaze Melt Fluidity
Use this novel device to compare the melt fluidity of glazes and materials. Simple physical observations of the results provide a better understanding of the fired properties of your glaze (and problems you did not see before).
Glossary Melt Fluidity
Ceramic glazes melt and flow according to their chemistry, particle size and mineralogy. Observing and measuring the nature and amount of flow is important in understanding them.
Tests Glaze Melt Fluidity - Ball Test
A test where a 10-gram ball of dried glaze is fired on a porcelain tile to study its melt flow, surface character, bubble retention and surface tension.
Tests Boiling Water:Ice Water Glaze Fit Test
Ceramic glazes that do not fit the body often do not craze until later. This test stresses the fit, thus revealing if it is likely to craze later.
Tests Frit Softening Point
In ceramics, this is the temperature at which a glaze or glass begins to flow, ceasing to exhibit the properties of a solid.
Tests Glaze Leaching Test
Simple tests to evaluate the stability of a ceramic or pottery glaze against leaching metals in food or drink.
Tests Glaze Hardness
Tests Glaze Observations
Typecodes Glaze Tests
Tests conducted on glaze batches used in production (as opposed to tests conducted on the materials used to make those glazes).

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy