44MR | APPO | AVPS | AVSC | BDGC | BDLB | BLOI | BWIW | CCON | CDRY | CEC | CLWC | CMST | COLE | COVB | CSSS | DENS | DFAC | DFDM | DIEL | DNLP | DS | DSHR | DSRN | DSTR | DTMP | EBCT | EM20 | FRFU | FRRD | FRTG | FSHR | FSTR | GBBT | GBMF | GEBR | GLAZ | GLFL | GLHD | GLLE | GSPT | GTTM | HDMI | | HMA | HMAN | HMOH | IFP | IWCT | L10M | L1M | L20M | L2M | L30M | L5 | L5M | LDW | LOI | LQLM | MDPS | MLRG | MOIP | MOR | MOR5 | MORD | OLAD | P200 | P325 | PBPO | PCE | pHPG | pHPW | PPD | PRSM | PSHP | RC | RHEO | SADR | SAMG | SCLE | SHAB | SIEV | SLBY | SOLU | SPHC | SSAB | SVWT | TGA | THCO | TNST | TREL | TRMN | TSFL | UPSD | WABS | WOPL | WRA | WSR | XREF

HEGF - Hegman Fineness Test

LSTM-17 test method.
This is quoted on talc and kaolin data sheets, for example.

Here is a good description of the method from gardco.com:
In its simplest conception, a Fineness of Grind Gage may be considered essentially a continuous variable screen. It can be readily seen that if a material such as fine silica were distributed uniformly in a single particle thickness in the gage path, these particles would protrude above the sides of the path starting at whatever point that their physical size exceeded the depth of the path.

If a straight edge scraper was brought to bear on the sides of the path in conjunction with the deepest part, and then moved slowly down the path to the shallow end, it would contact the protruding particles and on continued movement, screen or push these particles from the path.

Variables

VAL - Value (V)

Related Information

Links

URLs http://www.gardco.com/pages/dispersion/finessofgrind_gauges.html
Guardco Hegman Fineness Page
Tests Sieve Analysis Dry
A measure of particle size distribution by vibrating a powdered sample through a series of successively finer sieves
Tests Sieve Analysis Wet
A measure of particle size distribution by washing a powdered or slaked sample through a series of successively finer sieves
Tests Sieve Analysis 35-325 Wet
A measure of particle size distribution by washing a powdered or slaked sample through a series of successively finer sieves
Tests Wet Sieve Residue
Make a quick determination of oversize particles by washing a measured amount of powder through a 150 or 200 mesh sieve.
Typecodes Particle Tests
Tests conducted to determine particle populations, sizes, shapes, densities, surface areas, etc.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy