Alternate Names: Mno2, Pyrolusite, Manganese(IV) oxide, Manganese Oxide
Formula: MnO2
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| MnO2 | 100.00% | 1.00 | |
| Oxide Weight | 86.90 | ||
| Formula Weight | 86.90 | ||
This is available as a pure material or as a ground ore (pyrolusite). Thus while generically it is pure MnO2 the actual name-brand materials may only be 75% MnO2.
During firing, half of the oxygen disassociates to produce MnO (with an associated LOI of 14%). MnO is a flux. It reacts with silica to produce violet colors in the absence of alumina, browns in its presence.
Reactive and iridescent glazes commonly contain very high percentages of this material, 25% or even more (often in high feldspar base glazes). Additions of other metal oxides (e.g. copper oxide, cobalt oxide, iron oxide) further amplify the variegation and crystallization. Alberta Slip (formerly Albany Slip) makes an excellent base glaze (with added feldspar), it supplies the iron oxide and suspending properties. Multilayering with such glazes is very common among hobbyists and even potters.
Manganese dioxide is the key to Rockingham brown glazes which were made by employing about 3% iron oxide and 7% manganese in a transparent lead glaze of a recipe such as: Feldspar 28, Kaolin 14, Flint 4, Lead bisilicate 40, Whiting 4.
Manganese browns have a different, often more pleasant character than iron browns, especially in reduction firing.
Manganese, as the material of commerce, reduces through several forms during firing (i.e. Mn2O3, Mn3O4, Mn2O7) on its way to being converted to MnO by 1200C.
Pure manganese dioxide is often added to clay bodies to darken their fired color, 10% is typically enough for black (or half of that for grey). For lower temperatures (e.g. 1000C) most manufacturers would not worry about metal fumes during firing. But for cone 6 and above there is disagreement as to whether they are released.

This picture has its own page with more detail, click here to see it.

This picture has its own page with more detail, click here to see it.
The stains are still powders, showing their advantage over using raw metal oxides to color glazes. Pretty well all black glazes employ manganese along with other metal oxides, double or triple their combined percentage is needed to stain a glaze black. Much of the reason for this is that they dissolve in the melt.

This picture has its own page with more detail, click here to see it.
This bag will give you a clue as to what manganese dioxide, MnO2, is mainly used for. Staining bricks.

This picture has its own page with more detail, click here to see it.
These metal oxides have been mixed with 50% Ferro frit 3134 and fired to cone 6 oxidation. Chrome and rutile have not melted, copper and cobalt are extremely active melters, frothing and boiling. Cobalt and copper have crystallized during cooling. Manganese has formed an iridescent glass.

This picture has its own page with more detail, click here to see it.
Notice how the bubbling from the off-gassing of the manganese has variegated the surface.

This picture has its own page with more detail, click here to see it.
You add up to 5% manganese dioxide. The base recipe is G2571A. The clay body is a buff burning stoneware having iron speckle. The quality of the surface is excellent and it is durable.

This picture has its own page with more detail, click here to see it.
By Tony Hansen

This picture has its own page with more detail, click here to see it.
This glaze is 49% Wood Ash, 24% Soda Feldspar and 27% Ball Clay. 10 copper carbonate and 10 manganese dioxide are added to that. This beautiful sculpture was made by Dan Ingersoll, aesthetically this glaze is perfect for it. But there are two red flags here. Significant manganese and copper metal fumes are certain to be generated at cone 10 (they are seriously not healthy) so anyone using this must be very careful. But there is something much more serious - this glaze is being used on functional ware. Copper is well known to destabilize other metals in the fired glass. This 10:10 combination is a perfect storm for leaching heavy metal into food and drink. This is not an argument for the use of commercial glazes, it is one for common sense application of the concept of limit recipes.

This picture has its own page with more detail, click here to see it.
Laguna Barnard Slip substitute fired at cone 03 with a Ferro Frit 3195 clear glaze. The very high bubble content is likely because they are adding manganese dioxide to match the MnO in the chemistry of Barnard (it gases alot during firing).
| Hazards |
Manganese Toxicity by Elke Blodgett
A story of the struggle of one person to identify and deal with manganese toxicity |
| Hazards |
Manganese: Creativity and Illness by Dierdre O'Reilly
A story of one persons struggle with manganese toxicity |
| Hazards |
Manganese and Parkinsons by Jane Watkins
A story of one person and manganese poisoning. |
| Hazards |
Manganese Inorganic Compounds Toxicology
|
| Hazards |
Manganese in Clay Bodies
Manganese is used to stain clays (using black) and to impart fired speckling (as a decorative effect). It is dangerous? |
| URLs |
https://digitalfire.com/4sight/datasheets/SDSManganeseDioxide.pdf
SDS Prince Minerals Manganese Dioxide |
| Glossary |
Metal Oxides
Metal oxide powders are used in ceramics to produce color. But a life time is not enough to study the complexities of their use and potential in glazes, engobes, bodies and enamels. |
| Typecodes |
Colorant
Metallic based materials that impart fired color to glazes and bodies. |
| Typecodes |
Generic Material
Generic materials are those with no brand name. Normally they are theoretical, the chemistry portrays what a specimen would be if it had no contamination. Generic materials are helpful in educational situations where students need to study material theory (later they graduate to dealing with real world materials). They are also helpful where the chemistry of an actual material is not known. Often the accuracy of calculations is sufficient using generic materials. |
| Temperatures | Manganese dioxide decomposes to MnO (470-1200) |
| Materials |
Manganese Oxide
|
| Materials |
Manganese Carbonate
|
| Materials |
Manganese Granular
In ceramics, it is used primarily in clays and glazes to achieve fired speckle (including the brick industry). |
| Oxides | MnO2 - Manganese Dioxide |
| Oxides | MnO - Manganous Oxide |
| Minerals |
Manganite
Ore of manganese. |
| Minerals |
Hübnerite
A manganese mineral. |
| Density (Specific Gravity) | 4.9-5.0 |
|---|
| Body Color | When added to terra cotta bodies in amounts around 5% manganese dioxide will produce dark gray to black firing bodies. |
|---|---|
| Glaze Color | Large amounts of manganese can produce metallic effects in a glaze. However, these glazes must not be used on food surfaces. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk