Alternate Names: Frit 626, Frit P626
Description: Low fire high-barium leadless borosilicate
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| BaO | 27.40% | 0.66 | |
| Na2O | 5.60% | 0.34 | |
| B2O3 | 12.40% | 0.66 | |
| Al2O3 | 5.40% | 0.20 | |
| SiO2 | 49.20% | 3.04 | |
| Oxide Weight | 371.67 | ||
| Formula Weight | 371.67 | ||
Add 10% clay for cone 06-02 glaze.
This is a high barium frit (and thus can have issues with leaching in glazes if not used properly). If you got a recipe on line for a functional glaze and it contains a significant percentage of this, and the source does not mention the barium content, then contact them and complain. Substitutes include Fusion F-65) but they require industrial-sized orders and ceramic suppliers do not resell it. But Lagunaclay.com sells Ferro Frit 3289, it is the same chemistry. Another options is to calculate how to source the BaO from other sources (e.g. barium carbonate), keeping the overall chemistry of the glaze the same (using your account at insight-live.com).

This picture has its own page with more detail, click here to see it.
She was searching for a a matte, mottled white, rustic. For functional surfaces. And it contained this frit. The source from which she got it did not mention the barium content. Barium is certainly not a requirement to achieve a matte surface at cone 6, there of lots of ways to do it. And there are multiple matte mechanisms that can be exploited.
| Materials |
Ferro Frit 3289
|
| Materials |
Hommel Frit 400
|
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Materials |
Ferro Frit FB-284-M
|
| Materials |
Fusion Frit F-65
|
| Materials |
General Frit GF-129
|
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Hazards |
Barium Carbonate in Glazes
|
| Co-efficient of Linear Expansion | 7.2 x 10-6 (50-450C) |
|---|---|
| Frit Melting Range (C) | 1460-1570F |