A ChatBot gives jaw-dropping glaze recipe advice - Jan 2025
A Low Cost Tester of Glaze Melt Fluidity
A One-speed Lab or Studio Slurry Mixer
A Textbook Cone 6 Matte Glaze With Problems
Adjusting Glaze Expansion by Calculation to Solve Shivering
Alberta Slip, 20 Years of Substitution for Albany Slip
An Overview of Ceramic Stains
Are You in Control of Your Production Process?
Are Your Glazes Food Safe or are They Leachable?
Attack on Glass: Corrosion Attack Mechanisms
Ball Milling Glazes, Bodies, Engobes
Binders for Ceramic Bodies
Bringing Out the Big Guns in Craze Control: MgO (G1215U)
Can We Help You Fix a Specific Problem?
Ceramic Glazes Today
Ceramic Material Nomenclature
Ceramic Tile Clay Body Formulation
Changing Our View of Glazes
Chemistry vs. Matrix Blending to Create Glazes from Native Materials
Concentrate on One Good Glaze
Copper Red Glazes
Crazing and Bacteria: Is There a Hazard?
Crazing in Stoneware Glazes: Treating the Causes, Not the Symptoms
Creating a Non-Glaze Ceramic Slip or Engobe
Creating Your Own Budget Glaze
Crystal Glazes: Understanding the Process and Materials
Deflocculants: A Detailed Overview
Demonstrating Glaze Fit Issues to Students
Diagnosing a Casting Problem at a Sanitaryware Plant
Drying Ceramics Without Cracks
Duplicating Albany Slip
Duplicating AP Green Fireclay
Electric Hobby Kilns: What You Need to Know
Fighting the Glaze Dragon
Firing Clay Test Bars
Firing: What Happens to Ceramic Ware in a Firing Kiln
First You See It Then You Don't: Raku Glaze Stability
Fixing a glaze that does not stay in suspension
Formulating a body using clays native to your area
Formulating a Clear Glaze Compatible with Chrome-Tin Stains
Formulating a Porcelain
Formulating Ash and Native-Material Glazes
G1214M Cone 5-7 20x5 glossy transparent glaze
G1214W Cone 6 transparent glaze
G1214Z Cone 6 matte glaze
G1916M Cone 06-04 transparent glaze
Getting the Glaze Color You Want: Working With Stains
Glaze and Body Pigments and Stains in the Ceramic Tile Industry
Glaze Chemistry Basics - Formula, Analysis, Mole%, Unity
Glaze chemistry using a frit of approximate analysis
Glaze Recipes: Formulate and Make Your Own Instead
Glaze Types, Formulation and Application in the Tile Industry
Having Your Glaze Tested for Toxic Metal Release
High Gloss Glazes
Hire Us for a 3D Printing Project
How a Material Chemical Analysis is Done
How desktop INSIGHT Deals With Unity, LOI and Formula Weight
How to Find and Test Your Own Native Clays
I have always done it this way!
Inkjet Decoration of Ceramic Tiles
Is Your Fired Ware Safe?
Leaching Cone 6 Glaze Case Study
Limit Formulas and Target Formulas
Low Budget Testing of Ceramic Glazes
Make Your Own Ball Mill Stand
Making Glaze Testing Cones
Monoporosa or Single Fired Wall Tiles
Organic Matter in Clays: Detailed Overview
Outdoor Weather Resistant Ceramics
Painting Glazes Rather Than Dipping or Spraying
Particle Size Distribution of Ceramic Powders
Porcelain Tile, Vitrified Tile
Rationalizing Conflicting Opinions About Plasticity
Ravenscrag Slip is Born
Recylcing Scrap Clay
Reducing the Firing Temperature of a Glaze From Cone 10 to 6
Setting up a Clay Testing Program in Your Company or Studio
Simple Physical Testing of Clays
Single Fire Glazing
Soluble Salts in Minerals: Detailed Overview
Some Keys to Dealing With Firing Cracks
Stoneware Casting Body Recipes

Super-Refined Terra Sigillata
The Chemistry, Physics and Manufacturing of Glaze Frits
The Effect of Glaze Fit on Fired Ware Strength
The Four Levels on Which to View Ceramic Glazes
The Majolica Earthenware Process
The Potter's Prayer
The Right Chemistry for a Cone 6 Magnesia Matte
The Trials of Being the Only Technical Person in the Club
The Whining Stops Here: A Realistic Look at Clay Bodies
Those Unlabelled Bags and Buckets
Tiles and Mosaics for Potters
Toxicity of Firebricks Used in Ovens
Trafficking in Glaze Recipes
Understanding Ceramic Materials
Understanding Ceramic Oxides
Understanding Glaze Slurry Properties
Understanding the Deflocculation Process in Slip Casting
Understanding the Terra Cotta Slip Casting Recipes In North America
Understanding Thermal Expansion in Ceramic Glazes
Unwanted Crystallization in a Cone 6 Glaze
Using Dextrin, Glycerine and CMC Gum together
Volcanic Ash
What Determines a Glaze's Firing Temperature?
What is a Mole, Checking Out the Mole
What is the Glaze Dragon?
Where do I start in understanding glazes?
Why Textbook Glazes Are So Difficult
Working with children

Substituting Cornwall Stone

Description

Calculating a recipe of materials having the same oxide chemistry as Cornwall Stone

Article

Cornwall Stone is quite different from feldspars. Consider Custer Feldspar and Nepheline Syenite.

CaO MgO K2O Na2O TiO2 Al2O3 SiO2 Fe2O3LOI
Cornwall Stone 1.810.144.303.300.1516.3373.760.20  
Custer Feldspar 0.30 10.282.91 17.3569.000.12 0.04
Nepheline Syenite (Canada) 0.350.034.8010.60 23.5060.200.08  


Here is a wide range of analyses from data sheets and textbooks.

# MATERIAL WEIGHT CaO MgO K2O Na2O Fe2O3 TiO2 Al2O3 SiO2
100 NUMBER 1 640.93 0.21 0.06 0.29 0.43 0.01 0.01 0.97 7.72
101 NUMBER 2 682.90 0.23 0.03 0.34 0.37 0.01 0.02 1.02 8.27
102 NUMBER 3 680.57 0.29 0.02 0.27 0.40 0.00 0.02 1.06 8.19
103 NUMBER 4 705.21 0.27 0.02 0.32 0.37 0.01 0.02 1.10 8.47
104 NUMBER 5 717.95 0.22 0.04 0.32 0.40 0.01 0.02 1.09 8.73
105 NUMBER 6 696.23 0.22 0.02 0.16 0.59 0.00 0.01 1.11 8.45
106 NUMBER 7 718.73 0.27 0.04 0.31 0.36 0.01 0.01 1.13 8.66
107 NUMBER 8 736.85 0.28 0.04 0.31 0.35 0.01 0.02 1.12 8.97
108 NUMBER 9 1118.35 0.18 - 0.56 0.22 0.01 0.03 1.85 13.68
109 NUMBER 10 963.42 0.15 - 0.39 0.42 0.01 0.02 1.61 11.70
110 NUMBER 11 685.63 0.26 0.01 0.48 0.25 0.01 - 1.13 8.10
111 NUMBER 12 738.13 0.18 0.02 0.35 0.43 0.01 0.01 1.15 8.82


Fluorine has not been included. To get an average I entered each of these as a material into desktop Insight and added equal parts of each to a recipe. A detail report (below) reveals an average formula and recipe.

DETAIL PRINT - CORNWALL STONE AVERAGE
MATERIAL PARTS WEIGHT *CaO *MgO *K2O *Na2O *Fe2O3 *TiO2 Al2O3 SiO2
WEIGHT OF EACH OXIDE   56.10 40.30 94.20 62.00 160.00 79.70 102.00 60.00
NUMBER 1 500.00 640.93 .16 .05 .22 .33 .01 .01 .76 6.02
NUMBER 2 500.00 682.90 .17 .03 .25 .27 .01 .01 .74 6.06
NUMBER 3 500.00 680.57 .22 .01 .20 .29 .00 .01 .78 6.02
NUMBER 4 500.00 705.21 .19 .01 .23 .26 .01 .01 .78 6.00
NUMBER 5 500.00 717.95 .15 .03 .22 .28 .01 .01 .76 6.08
NUMBER 6 500.00 696.23 .16 .01 .11 .42 .00 .01 .79 6.07
NUMBER 7 500.00 718.73 .19 .02 .22 .25 .01 .01 .79 6.02
NUMBER 8 500.00 736.85 .19 .03 .21 .24 .01 .01 .76 6.09
NUMBER 9 500.00 1118.35 .08 - .25 .10 .01 .01 .83 6.12
NUMBER 10 500.00 963.42 .08 - .20 .22 .01 .01 .83 6.07
NUMBER 11 500.00 685.63 .19 .01 .35 .18 .00 - .82 5.90
NUMBER 12 500.00 738.13 .12 .01 .24 .29 .01 .00 .78 5.97
TOTAL 6000.00   1.90 .21 2.70 3.13 .07 .11 9.43 72.42
UNITY FORMULA   .23 .03 .33 .39 .01 .01 1.16 8.92
PER CENT BY WEIGHT   1.81 .14 4.31 3.30 .20 .15 16.33 73.76


Here is an example glaze recipe in which our L3617 Cornwall Stone substitute could be used..

WHITING............. 37.70
FERRO FRIT 3134..... 55.80
KAOLIN.............. 35.50
SILICA.............. 50.70
CORNWALL STONE...... 20.30
                     -----
                    200.00

There are two ways: Weigh up a batch of the Cornwall substitute, mix it thoroughly, then treat it as a raw material (if you are confident enough in being able to shake the mix enough in a plastic bag to believe it is mixed well). Otherwise, retotal the Cornwall substitute to 20.3 and combine it with the above recipe. Actually, both of these approaches have a small issue. The L3617 recipe contains materials have that an LOI, its total calculated LOI is 2.4%. That means the most correct amount to substitute for 20.3 is 20.3/(100-0.27/100) or 20.8.

Related Information

L3617 Cornwall Stone substitute vs. real Cornwall Stone


This picture has its own page with more detail, click here to see it.

This melt fluidity comparison demonstrates how similar the substitute L3617 recipe (left) is to the real material (right). 20% Frit 3134 has been added to each to enable better melting at cone 5 (they do not flow even at cone 11 without the frit). This substitute is chemically equivalent to what we feel is the best average for the chemistry of Cornwall Stone.

Two Cornwall Stone shipments compared to two substitutes


This picture has its own page with more detail, click here to see it.

This is a cone 11 oxidation melt flow test. Shown (left to right):
-A new shipment of Cornwall Stone 2011
-L3617 Digitalfire calculated substitute recipe
-An older Cornwall shipment
-The H&G substitute 2011 (far right, mislabelled on the picture).
These do not flow well here, a small frit addition was later employed to better compare them. However they have melted enough to see some differences in whiteness and degree of melt. Notice the L3617 is more like the old Cornwall Stone than the new Cornwall is.

Links

Materials Cornwall Stone

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy