Description: Potash/sodium/calcium Feldspar
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 1.05% | 0.15 | |
| K2O | 2.86% | 0.24 | |
| Na2O | 4.86% | 0.61 | |
| Al2O3 | 13.47% | 1.04 | |
| SiO2 | 77.37% | 10.10 | |
| Fe2O3 | 0.06% | - | |
| LOI | 0.07% | n/a | |
| Oxide Weight | 781.94 | ||
| Formula Weight | 782.49 | ||
Sil-O-Spar is a high quality blend of sodium/potassium/calcium aluminum silicate (feldspar) and silica, ground to 170 mesh, for ceramic applications. Carefully beneficiated and controlled for quality, Sil-O-Spar provides the advantages of pre-blended and uniformly sized non-plastic flux with low iron oxide content. Its coarse particle size makes it an ideal choice for casting slips.
| URLs |
http://www.zemex.com/feldspar/silospar.html
Silospar Data Sheet |
| Typecodes |
Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies. |
| Materials |
Soda Feldspar
A feldspar having a KNaO content that predominates in sodium. |
| Materials |
Potash Feldspar
A feldspar having a KNaO content that predominates in potassium. |
| Materials |
Calcium Feldspar
|
| Materials |
NC-4 Feldspar
|
| Materials |
G-200 Feldspar
|
| Materials |
G-20 Feldspar
|
| Materials |
F-20 Feldspar
|
| Apparent Viscosity (cps) | 14.37 |
|---|---|
| Bulk Density lbs/cu. ft. (Packed) | 37 loose, 87 packed |
| Sieve Analysis Dry | +200 mesh: 2.78% +325 mesh: 11.43% |
| Surface Area (m2/gm) | 1.13 |
| pH for dry powder | 9 |