Pemco Frit P-1J81

Alternate Names: P1J81,1J-81

Description: Semi-opaque all-fritted glaze for cone 02-4

Oxide Analysis Formula Tolerance
CaO 5.10% 0.23
K2O 8.60% 0.24
MgO 0.60% 0.04
Na2O 4.50% 0.19
ZnO 9.60% 0.30
ZrO2 3.20% 0.07
B2O3 4.80% 0.18
Al2O3 13.40% 0.34
SiO2 50.30% 2.16
Oxide Weight 258.25
Formula Weight 258.25

Notes

Add 10% clay.
Generally used with additional zirconium silicate opacifier. This glaze has excellent gloss and smoothness at Cone 02 through Cone 1.

Related Information

Links

Materials Pemco Frit P-991
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Pemco Frit P-3E12
Materials Ferro Frit 3820
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 8.40
Co-efficient of Linear Expansion 8.40 (50-450C)
Frit Softening Point 1620F
Frit Melting Range (C) 1580-1680F
Co-efficient of Linear Expansion 8.4x10-6 (50-450C)
I.F.P. (celsius) 610C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy