Ferro Frit 3269

Alternate Names: F3269

Description: Leadless high alkali low calcia frit

Oxide Analysis Formula Tolerance
CaO 0.41% 0.03
K2O 7.42% 0.29
Na2O 10.97% 0.64
ZnO 0.97% 0.04
B2O3 15.06% 0.79
Al2O3 12.40% 0.44
SiO2 51.23% 3.10
F 1.50% 0.29
Oxide Weight 363.58
Formula Weight 363.58

Notes

This is a USA pottery frit. Ferro now calls it Frit 3269-2.

Useful for partially fritted gloss tile glazes for cone 06-01. Balanced enough for use alone (if the application can tolerate its high thermal expansion). Like Frit 3110, the high expansion makes it suitable as a crackle glaze (with an addition of 10% kaolin).

Unlike Frit 3110, this has significant B2O3 and Al2O3 and almost no CaO.

Related Information

Links

Materials Fusion Frit F-225
Materials Hommel Frit 259
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials General Frit GF-114
Materials Fusion Frit FZ-25
Materials Ferro Frit 3819
Materials Hommel Frit 25
Materials Pemco Frit P-25
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.
URLs https://digitalfire.com/4sight/datasheets/ferropotteryfrits2008.pdf
Ferro Pottery Frits 2008

Data

Co-efficient of Linear Expansion 9.98
Frit Melting Range (C) 1400-1500F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy