1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Ferro Frit 3819

Description: Leadless high sodium frit for cone 06-02

Oxide Analysis Formula Tolerance
CaO 0.30% 0.02
K2O 7.20% 0.25
Na2O 13.00% 0.69
ZnO 1.00% 0.04
B2O3 16.60% 0.79
Al2O3 12.60% 0.41
SiO2 47.70% 2.61
F 1.60% 0.28
Oxide Weight 329.23
Formula Weight 329.23

Related Information

Links

Materials Hommel Frit 259
Materials Ferro Frit 3269
Materials Pemco Frit P-25
Materials Fusion Frit FZ-25
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 10.30
Co-efficient of Linear Expansion 10.3 x 10-6
Frit Softening Point 1400F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy