Description: Dark buff-firing plastic stoneware
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| K2O | 0.75% | 0.02 | |
| Al2O3 | 32.50% | 1.00 | |
| SiO2 | 52.00% | 2.72 | |
| Fe2O3 | 2.20% | 0.04 | |
| MgO | 0.60% | 0.05 | |
| CaO | 0.20% | 0.01 | |
| Na2O | 0.30% | 0.02 | |
| LOI | 11.20% | n/a | |
| Oxide Weight | 277.91 | ||
| Formula Weight | 312.96 | ||
It was first used in the late 1800s by Gladding McBean to make sewer pipe, subsequently for a wide range of architectural purposes. It is also used as a major ingredient in many commercial west coast USA stoneware and middle and high fire pottery clay and sculpture bodies. This material is very smooth and has a unique feel that many potters can recognize with their eyes closed!
Although this material is known as a fireclay, it completely vitrifies by cone 10 (where it is near zero porosity). it's porosity decreases steadily from cone 6 to 10, but it is beginning to bloat at cone 11. However, the fired shrinkage increases until cone 8 after which it bars begin to expand (indicating over firing). It would be an acceptable stoneware, by itself, at cone 7-8. With a 5% addition of feldspar it should be possible to make Lincoln fireclay work as a cone 6 stoneware. If crazing occurs blend in a high-silica cone 6 porcelain recipe (or a silica-feldspar mix with a little bentonite maintain plasticity).
Lincoln clay has several other very unusual properties also:
-It has excellent drying properties (resistance to cracking) even though it has high plasticity. It's drying shrinkage is below 6%.
-It is very plastic like a ball clay yet it feels like a kaolin (it is not sticky as are other clays of the same plasticity).
-27% water is required to make the Lincoln clay plastic enough to work for pottery (whereas a typical plastic pottery clay body is 20-22%). Yet it still has a fairly low during shrinkage! This is very unusual.
Variation in the physical and fired properties of this material have been a concern with its use in pottery. Its sieve analysis also varies considerably by batch. For this reason it is common to mix it with other materials to dampen an variation encountered.
This unique combination of firing behavior and workability made this an ideal material for making vitrified unglazed sewer pipe. Those same properties make it possible to create a pottery body having a very high percentage of this material (90% is feasible).
The ZAM stoneware pottery clay body has been made for many years by various manufacturers on the west coast. It is:
15 Hawthorn fireclay
10 Lincoln fireclay
40 Goldart
15 Ball clay
10 Silica
7 Feldspar
3 Redart
8 Grog or Sand
Another example is Soldner's Raku which is:
50 Lincoln fire clay
30 sand, all mesh
20 talc
It is also common to find recipes where Lincoln is blended with feldspar, silica and ball clay (where the ratios approximate or equal 50 ball clay, 25 silica, 25 kaolin). This is just a standard whiteware, so in effect, Lincoln is being blended with a porcelaneous stoneware.
Imco 400 Fireclay is similar to this material.

This picture has its own page with more detail, click here to see it.
The left two were made from a 100% mix of Lincoln 60, the right one adds 2% bentonite (Lincoln 60, by itself, matures into a stoneware at around cone 8). While it was possible to throw the pure material, the plasticity is a little lower than a normal pottery clay. That being said, it is smooth and has a soapy feel that makes it very pleasant to work with. A simple 2% addition of bentonite transformed it into a delight to throw! That only increased the drying shrinkage by about 0.5%. A potters wheel can thus be seen as a laboratory instrument, giving one the ability to make a comparative assessment like this (that no pairs of datasheets full of numbers will reveal).

This picture has its own page with more detail, click here to see it.
This is a Lincoln 60 fireclay drying disk (that has been fired to cone 10R). It has near zero-porosity and is dense and very strong. It is like a stoneware clay, quite vitreous.

This picture has its own page with more detail, click here to see it.
Materials are not always what their name suggests. These are Lincoln #60 Fireclay test bars fired at cone 10 reduction (top) and from cone 11 down to 6 oxidation (top to bottom). This clay already has stoneware density at cone 7 (3% porosity as indicated by our SHAB test). It vitrifies progressively from there upward (less than 3% porosity at cone 7 to near zero% by cone 9 oxidation. Maximum firing shrinkage happens at cone 8 and by cone 10 it is expanding (indicating decomposition has started) and it is bloating by cone 11 (melting is sealing the escape of gases of decomposition). Is Lincoln #60 a really fireclay? Absolutely not! But at cone 6 it is a credible plastic stoneware, all by itself!
| Materials |
Lincoln 8 Clay
|
| Materials |
Imco 400 Fireclay
|
| Materials |
Fireclay
|
| Typecodes |
Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically. |
| Typecodes |
Fireclay
Fireclays are non-kaolin non-ball clay materials similar to stoneware clays but lacking fluxing oxides. Many fireclays have a PCE of 28 or more. |
| URLs |
http://www.ceramicindustry.com/Articles/Feature_Article/f5877442bbac7010VgnVCM100000f932a8c0____
ZAM clay body recipe |
| Drying Shrinkage | 5.5-6.0% @ 27% water |
|---|---|
| Firing Shrinkage | Cone 6: 7.5% Cone 7: 8.0% Cone 8: 8.5% Cone 10: 8.0% |
| Pyrometric Cone Equivalent | 31 (claimed) |
| Sieve Analysis Dry | +35 mesh: 3.5 35-48: 3.0 48-65: 4.0 65-100: 3.5 100-150: 3.5 150-200: 4.0 200-325: 5.0 |
| Water absorption | Cone 6: 3.0% Cone 7: 2.5 Cone 8: 1.5 Cone 10: 0.2 |