Royal Ball Clay

Description: Legacy ball clay from United Clay Mines

Oxide Analysis Formula Tolerance
SiO2 52.80% 3.10
Al2O3 28.90% 1.00
Fe2O3 0.90% 0.02
TiO2 1.70% 0.08
CaO 0.20% 0.01
MgO 0.30% 0.03
K2O 1.70% 0.06
Na2O 0.30% 0.02
LOI 13.20%n/a
Oxide Weight 306.35
Formula Weight 352.94

Related Information

Links

Materials Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries.
Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

Data

% < 0.5 microns 36.1%
Firing Shrinkage 9.5% at cone 9
Dry M.O.R. (50% Silica) 510 psi

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy