1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Pemco Frit Pb-1279

Alternate Names: Frit Pb1279

Description: Very low lead barium frit for partially fritted glazes cone 04-5

Oxide Analysis Formula Tolerance
BaO 4.10% 0.06
CaO 6.90% 0.29
K2O 3.50% 0.09
MgO 2.00% 0.12
Na2O 5.10% 0.19
PbO 3.40% 0.04
ZnO 7.60% 0.22
B2O3 2.10% 0.07
Al2O3 12.70% 0.29
SiO2 52.60% 2.05
Oxide Weight 233.98
Formula Weight 233.98

Related Information

Links

Materials Fusion Frit FZ-6
Materials Ferro Frit 3560
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Hommel Frit 482
Typecodes Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 7.5 x 10-6 (50-450C)
Frit Softening Point 1600F
Frit Melting Range (C) 1550-1940F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy