1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Old Hickory FC340 Ball Clay

Alternate Names: FC-340 Ball Clay

Oxide Analysis Formula Tolerance
SiO2 62.04% 4.37
Al2O3 24.10% 1.00
Fe2O3 1.01% 0.03
TiO2 1.27% 0.07
CaO 0.05% -
MgO 0.30% 0.03
K2O 1.18% 0.05
Na2O 0.11% 0.01
LOI 9.94%n/a
Oxide Weight 381.17
Formula Weight 423.24

Notes

It is an equivalent to CDI ball clay used in talc casting slips.
It is a little more plastic that KT#1-4.

Related Information

Links

URLs http://www.oldhickoryclay.com/FC-340.htm
FC-340 Data Sheet
Materials Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries.
Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy