Alternate Names: Alkalifritte C-1233, Alkalifritte M 1233, Fritte M1233
Description: Very high alkali, zero boron, low alumina, high expansion frit
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 7.75% | 0.30 | |
| Na2O | 11.42% | 0.40 | |
| SiO2 | 66.41% | 2.40 | |
| K2O | 13.01% | 0.30 | |
| Al2O3 | 1.41% | 0.03 | |
| Oxide Weight | 217.18 | ||
| Formula Weight | 217.18 | ||
Commonly used to make crystalline glazes because of the very high alkali and very low alumina contents.
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Materials |
Degussa Frit 90208
|
| Materials |
Moulin Fritte M1233
|
| Materials |
Glasurfritten M1233
|
| Materials |
Fusion Frit F644
|
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Typecodes |
Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out. |
| Frit Softening Point | 503C |
|---|
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk