Alternate Names: Fusion Frit F-644
Description: Very high sodium, boron free, low alumina, high expansion frit
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| Na2O | 29.43% | 1.00 | |
| Al2O3 | 5.94% | 0.12 | |
| SiO2 | 64.63% | 2.27 | |
| Oxide Weight | 210.67 | ||
| Formula Weight | 210.67 | ||
Used in crystalline glazes. Very high thermal expansion.
This material is highlighted in the video: A Broken Glaze Meets Insight-Live and a Magic Material (link is provided on this page).
This frit has an incredibly high Na2O content coupled with very low Al2O3, that makes it potentially very useful in fixing glazes lacking sufficient clay content to suspend and harden them (substituting this enables lowering the feldspar and introducing clay to supply the lost Al2O3, for example). Ferro Frit 3110, commonly used in crystal glazes for its high KNaO, only has half as much as this! And for many applications Frit 3110 has unwanted B2O3.
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Materials |
Ferro Frit 3110
High sodium, high thermal expansion low boron frit. A super-feldspar in clay bodies. Melts at very low temperatures. Useful to make crackle glazes. |
| Materials |
Degussa Frit 90208
|
| Materials |
Mondre and Manz Frit 1233
|
| Media |
A Broken Glaze Meets Insight-Live and a Magic Material
Use Insight-Live.com to do major surgery on a feldspar saturated cone 10R glaze recipe with multiple issues: blistering, pinholing, crazing, settling, dusting and possibly leaching! |
| URLs |
http://www.fusionceramics.com/
Fusion Ceramics Frit Website |
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk