1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Foundry Hill Creme

Alternate Names: New Foundry Hill Creme, Foundry Hill Cream, Foundary Hill Cream

Description: Plastic clay for stoneware clay bodies

Oxide Analysis Formula Tolerance
CaO 0.50% 0.04
K2O 0.70% 0.04
MgO 0.50% 0.06
Na2O 0.55% 0.04
TiO2 0.50% 0.03
Al2O3 20.50% 1.00
P2O5 0.09% -
SiO2 66.20% 5.48
Fe2O3 1.60% 0.05
LOI 8.20%n/a
SO3 0.09%n/a
Oxide Weight 453.48
Formula Weight 494.47

Notes

Similar to a ball clay but having a much lower drying shrinkage (about 6-6.5%) and more iron (but a distinctly low TiO2). Although this is a fairly refractory clay, it has a high firing shrinkage, around 8% across the entire range from cone 7 to 11. Porosity drops slowly from cone 7 upward (7% down to 4% at cone 11 oxidation and 10 reduction). Used commonly in stoneware clay bodies.

The manufacturer states: An intermediate-grained engineered blend offering excellent moisture retention and plasticity properties. Ideally suited for a wide variety of stoneware applications and wet forming process.

Relative Viscosity (1.2 Sp. Gr.):* 1.28
Casting Rate: (gms per 15 min/426 cm2):* 209
Water of Plasticity:* 22.9
% Dry Shrinkage:* 3.94
Dry M.O.R., psi:* 239

Cone 04 8 11
----
Fired Shrinkage:* 0.2% 1.6% 1.9%
Absorption:* 20.2% 17.8% 15.2%
M.O.R. psi:* 758 2390 4630

Thermal Expansion, Cone 8: .493% at 700C
P.C.E.: 30
pH: 5.9
Oil Absorption: 28
Bulk Density, lbs per cubic foot: 37-45
Particle Size, Microns: 20 10 5 2 1 0.5 0.2
88% 73% 60% 44% 33% 21% 8%

*Specimens: De-aired, extruded, 50% ball clay, 50% flint

Related Information

Original Container bag of Foundry Hill Cream clay


This picture has its own page with more detail, click here to see it.

Foundry Hill Creme fired test bars


This picture has its own page with more detail, click here to see it.

Top: Cone 10R (soluble salts are staining the surface). Downward: Cone 11-7 oxidation.
These look very similar to a typical ball clay, perhaps not firing quite as white.

In clay body testing it is about the data.

It reveals how a 20% feldspar addition affects this clay


Fired bars of foundry hill creme clay

This picture has its own page with more detail, click here to see it.

Foundry Hill Creme (FHC) is used in North America as a stoneware body base or addition. It fires like a ball clay but it is less plastic. How much feldspar would it take to make it into a vitreous cone 6 stoneware? I fired SHAB test bars from cone 4 to 10 (bottom to top) and 10R (the soluble salts discolor it in reduction). The data collected (in an Insight-live.com group account) produces firing shrinkage and absorption data that calculates to the red columns (and plots to the blue lines). Notice how the porosity drops steadily from cone 3 to 10 (the firing shrinkage rises steadily over the same period). A 20% nepheline syenite addition plots to the orange lines. Notice 2200F (cone 6): The porosity drops from 8% to vitreous (zero) while the firing shrinkage increases 2%. The FHC drying shrinkage (the first DSHR red column) averages 0.3% lower than the mix; this is counterintuitive but a pleasant surprise. While the mix did have a higher water content (which would increase drying shrinkage), another factor appears to be how well this clay hosts the feldspar addition without compromising its own plasticity.

Links

Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.
Materials Gleason Ball Clay

Data

Pyrometric Cone Equivalent 31

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved