1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Ferro Frit 5301

Alternate Names: F5301, Frit 501E34, Frit 5301-2

Description: Very high expansion leadless fluorine frit

Oxide Analysis Formula Tolerance
CaO 2.36% 0.13
K2O 5.53% 0.18
Na2O 14.03% 0.69
B2O3 12.48% 0.55
Al2O3 12.08% 0.36
SiO2 44.49% 2.26
F 9.00% 1.45
Oxide Weight 305.66
Formula Weight 305.66

Notes

This is a USA pottery frit, Ferro now calls it Frit 5301-2.
Formerly Frit 4101. This was probably originally a porcelain enamel frit since it has a very high thermal expansion and a lot of fluorine (they need formulations that melt at very low temperatures).

The high expansion makes it useful in crackle glazes at 06 or to counter shivering in other glazes.

Related Information

Links

Materials Fusion Frit F-102
Materials Ferro Frit 4194
Materials Ferro Frit 5325P
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Pemco Frit P-1084
Materials Ferro Frit 1012
URLs https://digitalfire.com/4sight/datasheets/ferropotteryfrits2008.pdf
Ferro Pottery Frits 2008
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 11.41 (50-450C)
Frit Melting Range (C) 1400-1500F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy