Alternate Names: F3292
Description: Strontium frit all or partially fritted clear glazes
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 10.53% | 0.54 | |
| K2O | 3.14% | 0.10 | |
| Li2O | 0.42% | 0.04 | |
| MgO | 0.70% | 0.05 | |
| Na2O | 3.01% | 0.14 | |
| SrO | 4.83% | 0.13 | |
| B2O3 | 5.75% | 0.24 | |
| Al2O3 | 10.76% | 0.30 | |
| SiO2 | 60.86% | 2.91 | |
| Oxide Weight | 287.63 | ||
| Formula Weight | 287.63 | ||
This is a USA pottery frit, Ferro now calls it Frit 3292-2.
Useful addition to first fire sanitary ware. Balanced, can make up the bulk of a recipe.
| Materials |
Fusion Frit F-134
|
| Materials |
Hommel Frit 389
|
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| URLs |
https://digitalfire.com/4sight/datasheets/ferropotteryfrits2008.pdf
Ferro Pottery Frits 2008 |
| Co-efficient of Linear Expansion | 7.62 |
|---|---|
| Frit Softening Point | 1650-1900F |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk