CGS 3.1 Spodumene

Description: Glass Grade Spodumene

Oxide Analysis Formula Tolerance
Li2O 5.00% 0.96
Fe2O3 0.10% -
Al2O3 18.50% 1.03
SiO2 75.00% 7.11
Na2O 0.25% 0.02
K2O 0.35% 0.02
LOI 0.30%n/a
Oxide Weight 565.14
Formula Weight 566.84

Notes

This is a lithium concentrate, not a commercial product. Talison Lithium primarily produces hard-rock lithium mineral concentrates (spodumene) at its Greenbushes mine in Western Australia. The company extracts and processes raw ore into two main categories of lithium concentrate and sells them directly to customers rather than producing refined lithium chemicals itself.
Technical-Grade Lithium Concentrates Features: Low iron content.Uses: Manufacture of ceramics, specialty glass, and heat-proof cookware.
Chemical-Grade Lithium Concentrates Features: High-yielding lithium mineral concentrate.Uses: Processed further into lithium chemicals (such as lithium hydroxide and lithium carbonate) to power lithium-ion batteries in electric vehicles, laptops, and mobile phones, as well as large energy grid storage systems.

Related Information

Links

URLs http://www.amalgamet.com/Products/minerals.htm
Description of material
Materials Spodumene Concentrate
Materials Foote Spodumene
Materials Spodumene
Spodumene is a lithium sourcing feldspar, an alternative to lithium carbonate to supply Li2O to ceramic glazes. Contains up to about 8% Li2O.
Materials Australian Spodumene
Typecodes Flux Source
Materials that source Na2O, K2O, Li2O, CaO, MgO and other fluxes but are not feldspars or frits. Remember that materials can be flux sources but also perform many other roles. For example, talc is a flux in high temperature glazes, but a matting agent in low temperatures ones. It can also be a flux, a filler and an expansion increaser in bodies.

Data

Hardness (Moh) 6-5-7
Frit Softening Point 1420C
Sieve Analysis Dry Tyler 150 mesh: 95%
Density (Specific Gravity) 3.2

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.