Hectalite 200

Alternate Names: Hectalite

Description: Dry processed Hectorite

Oxide Analysis Formula Tolerance
CaO 12.10% 0.27
K2O 0.33% -
MgO 20.30% 0.62
Na2O 2.80% 0.06
Al2O3 1.58% 0.02
SiO2 60.80% 1.25
Fe2O3 1.23% 0.01
Li2O 1.29% 0.05
LOI 8.50%n/a
Oxide Weight 123.78
Formula Weight 135.28

Notes

A plastic magnesium-rich sodium hectorite clay of microfine particles (it is a refined version of the same material from which HPM20 and Volclay bentonite are made).

Hectalite is available in grades 200 and GM, they have the same chemistry and other physical data except:
-Hectalite 200 has a viscosity of 2000-5000 cps @ 5% solids whereas GM is 50 cps.
-GM has a slightly lower pH of 8-10 whereas 200 is 9-11.
Hectalite 200 is intended for rheology control (stabilizing, gelling, suspending and binding household products, aerosols, paints, enamels and ceramic slurries) whereas Hectalite GM is intended for binding and plasticizing in ceramic bodies.

The high MgO, CaO, low Al2O3 and the presence of Li2O give this material a chemistry that is unlike other typical fine-particled clays.

Brightness: 70 minimum
Density: 2.6 g/cubic cm
Texture: Soft, slippery
Color: White to off-white

Wet Particle Size:
Through 200 mesh: 99.75%
Through 325 mesh: 99.0%

Moisture %, Maximum: 12%
pH (2% slurry): 9.0-11.0
LOI: 18.65

Specific to GM:
Free Swell: Minimum 24 mls
Viscosity: 2000 - 5000 @ 5% solids
pH: 8.0-10.0 @ 2% solids

CAS No. 1302-78-9

Related Information

Two plasticizers show vastly different potency


This picture has its own page with more detail, click here to see it.

A comparison of the plasticity of two bentonites was done by diluting them with silica. The top sample is Volcay 325 mixed 25:75 with silica. It is a standard Wyoming sodium bentonite - mined, dried and ground. The bottom specimen is Hectalite 200, a highly refined white hectorite, mixed 50:50 with silica. Notice how much less plastic it is (even though at double the percentage).

Links

Materials Magnabrite
Materials Polargel
Materials Volclay Bentonite
Materials Hectabrite
White magnesium-rich surface-modified highly purified sodium hectorite clay 4-5 times more efficient than raw bentonite.
Materials Bentolite L-3
Materials Bentonite
Bentonite can make a clay body instantly plastic, only 2-3% can have a big effect. It also suspends slurries so they don't settle out and slows down drying.
Materials Hectalite GM
Materials Hectorite
A sodium magnesium montmorillonite that burns much whiter than bentonite (because of lower iron content).
Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.