Alternate Names: Volclay 325 Bentonite, Dioctahedral smectite
Description: 364CER,334,355,660,149,446,105,356,840,331,351
Formula: (Na,Ca)0.33 (Al1.67Mg0.33)Si4O10(OH)2 nH2O
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.65% | 0.10 | |
| Na2O | 2.57% | 0.35 | |
| MgO | 2.67% | 0.56 | |
| FeO | 0.35% | 0.04 | |
| Fe2O3 | 3.25% | 0.17 | |
| Al2O3 | 21.08% | 1.73 | |
| SiO2 | 63.02% | 8.79 | |
| LOI | 5.64% | n/a | |
| Oxide Weight | 784.55 | ||
| Formula Weight | 831.44 | ||
A micronized sodium bentonite.
The 325 mesh version of this is most suitable for porcelains and a possible substitute for the more expensive HPM-20 Volclay.
Dioctahedral smectite, an expanding layer silicate.
Gray and cream-colored clays (montmorillonites) for use as suspension agents, viscosifiers, gellants and binders.
Has lower iron content that HPM-20 bentonite.
However while they company refers to their 325 mesh product, the data sheet says that 90% passes 325 mesh?

This picture has its own page with more detail, click here to see it.
The stated particle size of a material and fired appearance can both be misleading. For example, these are Volclay 325 bentonite particles fired to cone 8 oxidation. They are from a water washed sieve analysis test, the oversize particles from a 325 mesh screen (left) make up 2% of the total and 1% are from the 200 mesh screen (right). Although the 325 particles appear ominously dark, individually they are likely to small to produce apparent fired specks in a porcelain. However 200 mesh sizes can produce visible fired specks, but that fraction of oversize does not have nearly as high iron or flux content. Still, the finer darker particles could agglomerate, it might be better to use a cleaner bentonite to plasticize a porcelain.

This picture has its own page with more detail, click here to see it.
A comparison of the plasticity of two bentonites was done by diluting them with silica. The top sample is Volcay 325 mixed 25:75 with silica. It is a standard Wyoming sodium bentonite - mined, dried and ground. The bottom specimen is Hectalite 200, a highly refined white hectorite, mixed 50:50 with silica. Notice how much less plastic it is (even though at double the percentage).
| Materials |
Hectalite 200
|
| Materials |
Hectabrite
White magnesium-rich surface-modified highly purified sodium hectorite clay 4-5 times more efficient than raw bentonite. |
| Materials |
HPM-20 Volclay Bentonite
|
| Materials |
Fuller's Earth
|
| Typecodes |
Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically. |
| URLs |
http://www.colloid.com/ISG/TechData/Volclay%20325%20Mesh%20Tech%20Sheet.pdf
Volclay 325 Data Sheet |
| % Passing 325 Mesh Wet | 90% |
|---|---|
| Apparent Viscosity (cps) | 12 cps minimum @ 6.25% solids |
| pH for dry powder | 8.5-10.5 @ 5% solids |
| % Passing 200 Mesh Wet | 97% |