F-20 Feldspar

Alternate Names: F20 Feldspar

Description: Potash/sodium/calcium 20 mesh Feldspar

Oxide Analysis Formula Tolerance
CaO 1.40% 0.14
K2O 4.10% 0.24
Na2O 6.82% 0.62
Al2O3 18.85% 1.04
SiO2 68.15% 6.35
Fe2O3 0.07% -
LOI 0.08%n/a
Oxide Weight 556.87
Formula Weight 557.32

Notes

F-20 Feldspar is a high quality sodium/ Potassium/calcium aluminum silicate used principally as a flux for ceramic applications. Carefully beneficiated using the froth flotation process, F-20 Feldspar offers high levels of alkali oxides per unit of alumina with low iron oxide content.

Suitable for all types of glazes
Max Firing Temp: over 1250C

Related Information

Links

Materials Sil-o-spar
Materials G-20 Feldspar
Materials G-200 Feldspar
Materials Potash Feldspar
A feldspar having a KNaO content that predominates in potassium.
Materials Soda Feldspar
A feldspar having a KNaO content that predominates in sodium.
Typecodes Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies.
URLs https://www.thequartzcorp.com/assets/file/F_20_PDS.pdf
F-20 Feldspar data sheet

Data

Bulk Density lbs/cu. ft. (Packed) 80
Sieve Analysis Dry Cumulative: +30 mesh 1.8 +40 mesh 15.9 +200 mesh 94.7 -200 mesh 5.3
By Tony Hansen