Description: WBB Devon Ball Clay Group 4
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.20% | 0.02 | |
| K2O | 1.80% | 0.10 | |
| MgO | 0.30% | 0.04 | |
| Na2O | 0.20% | 0.02 | |
| TiO2 | 1.60% | 0.11 | |
| Al2O3 | 19.00% | 1.00 | |
| SiO2 | 71.00% | 6.34 | |
| Fe2O3 | 0.70% | 0.02 | |
| LOI | 5.30% | n/a | |
| C | 0.10% | n/a | |
| Oxide Weight | 508.93 | ||
| Formula Weight | 537.98 | ||
Particle Size (e.s.d.)
125 microns - 0.80
10 microns - 85
2 microns - 59
1 microns - 50
Modulus of Rupture at 110C
Mn/M2 - 6.9
lbf/in2 - 1000
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.2
Water Absorption
1120C - 5.5
1220C - 3.00
Shrinkage Dry to Fired
1120C - 6.50
1220C - 8.50
Reflectance 464nm
1120C - 63
1220C - 46
Refractoriness
Cone - 26, 1580C
| Materials |
Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries. |
| Typecodes |
Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites. |