Black Coring
Bleeding Colors
Bloating
Casting Slip Problems
Chrome Flashing in Ceramic Glazes
Clouding in Ceramic Glazes
Cracking of Clays During Drying
Crawling
Dunting and Cracking of Clay Bodies During Firing
Foaming of Ceramic Glaze Slurries
Glaze Blisters
Glaze Crazing
Glaze is Off-Color
Glaze Marks or Scratches
Glaze peeling on drying
Glaze Pinholes, Pitting
Glaze Shivering
Glaze Slurry is Difficult to Use or Settling
Leaking of Fired Ceramics
Lime Popping
Orange Peel Surface
Over Firing of Ceramic Glazes and Bodies
Powdering, Cracking and Settling Glazes
Runny Ceramic Glazes
Specking on Ceramic Ware
Splitting at the Plastic Stage
Staining of Fired Ceramic Glazes
Uneven Glaze Coverage
Warping

Dunting and Cracking of Clay Bodies During Firing

Ceramic industry can fire much faster and deal with much heavier objects than potters can, how do they do it. The answer is they pay more attention to the basics, it is all common sense and good equipment.

Details

At the Medalta Potteries (in Medicine Hat, Alberta, Canada) during the 1920s they made stoneware crocks up to 60 gallons. These monsters weighed more than 200 pounds and had walls between one and two inches thick. These crocks were made from the same clays that are employed in Plainsman H550 functional stoneware today and the glaze was typical of the feldspar recipes we still use. Even if you could fabricate one of these and figure out how on earth they dip-glazed a 250 pound unbisqued vessel, it would certainly crack into many pieces as it split during firing heat up and dunted during cooling. What was the firing secret? Simple. Energy was cheap, huge beehive kilns the size of a house could be fired for less than a dollar a month! Kilns were hard brick and massive and the firing cycle was one week. That's right, seven days. To me the moral of this story is that firing needs to be tuned to the ware.

Consider another case that the average potter would find equally mystifying. In industry today it is common for roller kilns to fire stoneware in a 2-3 hour cold-to-cold cycle. My experience tells me that this is impossible. How do they do it? Obviously, they can only do this with ware that is lighter. But still, it is amazing, there must be much more to it. Here are a few factors:

First, they use a body that employs low lignite, large particle, lower plasticity clays in the lowest possible proportion so water and gases can be vented out quickly.

Second, they fire smarter. There are firing consultants in industry that do nothing but design custom firing curves for manufacturers. In the firing of any body there are periods when temperature rise can be much faster and others when it must be slower. But how much faster and where? A thermo-gravimetric analysis (TGA) test weighs a clay sample during firing to determine when it expels the most gases. A differential thermal analysis (DTA) test reveals the periods of firing where the body is exothermic and where it is endothermic. With this and other information one can design a firing curve that provides for the shortest possible firing time.

Third, commercial kilns fire very evenly, some expose ware to less than a degree of gradient. Draft is one factor, many kilns have burners that double as blowers and create a kind of 'hurricane' within the kiln that exposes every part of ware to heat.

A fourth factor is not directly related to cracking but I will mention it. Modern glazes are formulated to be fast-fire. They are low in boron and remain unmelted until just before the end of the firing. This makes allowance for easy channeling of gases of body decomposition before the glaze melts.

How long should a firing be? If ware is cracking and you don't want to get into complicated analysis of your firing curve then it should just be longer, it is a relative thing. However it does not take brain surgeons to fire smarter also. Hold at boiling point as long as possible (over night candling is best) and go up (and especially down) through quartz inversion slower (1050F, 570C). In electric kilns there is no draft, this is a real problem in avoiding gradients; you have no choice but fire slower in the hopes of getting a more even firing.

Related Information

Bricks and tiles are cracking out of the kiln. How to solve this problem?


Cracking bricks out of kiln

This picture has its own page with more detail, click here to see it.

With data. Consider all the possible reasons. Die design not knitting clay together around floating elements; faulty deairing on the pugmill; clay too short to pug through the complex die, too soft or too stiff, lacks fine particle sizes, lacks dry strength; uneven or incomplete drying; too many sharp concaves or uneven thicknesses on the cross-section; kiln setting does not enable heat exposure to all surfaces; firing too uneven or too fast. Most of these properties can be measured, photographed and logged, and changes will thus be noticed. At a minimum, the SHAB test, LDW test and SIEV test and associated notes and photos will accumulate data to assist. These tiles are being made in the oldest city on earth, from the same clays as ancient Sumerian’s made their ziggurats!

Serious cracking in a crystalline-glazed P700 Grolleg porcelain. Why?


Three cracked crystal glazes porcelain vases

This picture has its own page with more detail, click here to see it.

The cracks appear to have happened on heat-up (because they have widened). Bisque firing was done around cone 04. Issue 1: The cone 10 electric firing was up-ramped at 400F/hr to 2330F (so it whizzed pass quartz inversion on the way!). Issue 2: Wall thickness variations in the pieces, they produce temperature gradients that widen as firing proceeds. Issue 3: Abrupt contour changes and sharp corners, especially when coincident with thickness variations, provide failure points that rapid temperature changes exploit. Issue 4: This new body is more plastic than the previous Grolleg porcelain used, that was likely an enabler to making these thin wall sections even thinner. But remember, practically any piece (unless it has huge in-stresses from uneven drying) can exit a kiln crack-free if firing is done evenly and slowly enough. Results of past firings are the main guide to know what to do in future ones, this is now a "past firing". So the first obvious fix here is slower heat-up, especially around quartz inversion (1000-1100F). Second: more even wall thickness.

Here is what happens when you fire a heavy, thick piece in an electric kiln


This picture has its own page with more detail, click here to see it.

The heat-up was not slow enough. This kiln has no air flow. This piece was very thick. What would it take to fire this? Possibly days of holding at 250F to drive off pore water. Then days of slow heat up.

Cracking casseroles. Why?


An upside down cracked casserole dish

This picture has its own page with more detail, click here to see it.

The cracks happened on heat up (since they have opened up wide). A combination of issues contribute. The kiln shelves heat-sink the wide flat bottoms, vessel walls are thick, there is some unevenness of wall thickness and only a 30-minute hold at 220F to remove glaze water from the bisque (that could have left dampness in thicker sections). Factors like these combine to produce temperature gradients within the piece. The firing schedule rose rapidly from 250-2100F (400F/hr) amplifying these gradients as it climbed. At quartz inversion these gradients produced a wave of volumetric change moving through the bisqued piece and this likely initiated a crack where stresses met at a combination sharp-contour and thickness-change, the bottom corner.

Cross section is an important factor in avoiding cracks


This picture has its own page with more detail, click here to see it.

The cross section of a bowl. For the best success in drying and firing, it is advantageous to have as even of a thickness as possible. But it is also important not to have sharp concave angles. It would have been possible to make the section outside the foot ring thinner by creating a more abrupt concave contour, but that contour, if too sharp, could offer a point of weakness where a crack could start.

This horizontal crack began as stresses created during uneven drying


This picture has its own page with more detail, click here to see it.

The rim was allowed to get ahead of the base. A thinner section (that happened during throwing) was exploited by the stresses and a crack appeared during heatup, likely during the bisque.

This crack likely starting during bisque


This picture has its own page with more detail, click here to see it.

It started at a sharp angled indent on the outside (that coincided with a thin wall section) and grew around the perimeter (not visible). From there it branched to the base.

Tile having angular shape is cracking at vertexes


This picture has its own page with more detail, click here to see it.

Cracks are happening during heatup (we know this because these have widened, cooling cracks are hairlines). Assuming the cracks were not there after drying, the piece likely could have been fired successfully by employing a slower heat-up. How to solve: Smooth, compress and round those sharp concave angles. This denies cracks a place to start. Even if the concave corners could have been rounded and compressed to a tiny radius (e.g. 2mm), it would likely have helped. And rounding and compressing the sharp edges would help (there are a couple of cracks on the straight sides).

Cracking from the rim during bisque:

Uneven heat-up or cool-down can do this


A casserole dish with a dunting crack going down from the rim

This picture has its own page with more detail, click here to see it.

This crack is characteristic of a firing dunt: stresses created when different parts of the piece are changing temperature, and therefore dimensions, at different rates. When those stresses exceed the strength of the body, a crack releases them. The quartz inversion around 570C is especially important - a temperature difference across the piece at this point means one area can be undergoing the quartz volume change while another is not.

Large, heavy pieces and those having uneven cross sections develop temperature gradients more readily. This piece has another disadvantage: its wide flat bottom is coupled thermally to a heavy kiln shelf while the vertical walls are much more directly exposed to radiant heat. That can produce substantial temperature differences during both heating and cooling, especially if one side faces the elements more directly. Slowing the firing through quartz inversion, on both the way up and the way down, and avoiding uneven radiant exposure can greatly reduce the risk.

22 inch slabs successfully fired after a change. What?


22 inch tiles successfully being fired

This picture has its own page with more detail, click here to see it.

Giant thin meter-square tiles are fired flat and crack-free by tile companies. How? Kilns that heat evenly from above and below (the tiles are on rollers). But these round tiles are being fired in an electric kiln, a device incapable of heating a large slab evenly. They are so large they reach almost to the outer walls. That means the outer edges receive direct radiant heat from the elements, this sets up a temperature gradient running from the edges toward the center. Passing such a piece up and down through quartz inversion thus creates a wave of sudden expansion and contraction moving through the piece. The artist was losing every one of these to dunting. It is not really advisable to even try this - but he was determined to do it anyway. One change in the process brought this one through: Slowing down to 50F/hr up and down through the quartz inversion (950-1150F).

Links

Articles Some Keys to Dealing With Firing Cracks
Ceramic industry can fire much faster and deal with much heavier objects than potters can, how do they do it. The answer is they pay more attention to the basics, it is all common sense and good equipment.
Projects Firing Schedules

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy