44MR | APPO | AVPS | AVSC | BDGC | BDLB | BLOI | BWIW | CCON | CDRY | CEC | CLWC | CMST | COLE | COVB | CSSS | DENS | DFAC | DFDM | DIEL | DNLP | DS | DSHR | DSRN | DSTR | DTMP | EBCT | EM20 | FRFU | FRRD | FRTG | FSHR | FSTR | GBBT | GBMF | GEBR | GLAZ | GLFL | GLHD | GLLE | GSPT | GTTM | HDMI | HEGF | HMA | HMAN | HMOH | IFP | IWCT | L10M | L1M | L20M | L2M | L30M | L5 | L5M | LDW | LOI | LQLM | MDPS | MLRG | MOIP | MOR | MOR5 | MORD | OLAD | P200 | P325 | PBPO | PCE | pHPG | pHPW | PPD | PRSM | PSHP | RC | RHEO | SADR | SAMG | SCLE | SHAB | SIEV | SLBY | SOLU | SPHC | SSAB | SVWT | TGA | THCO | TNST | TREL | TRMN | TSFL | UPSD | WABS | WOPL | WRA | WSR | XREF

BLOI - Borate LOI Test

The LOI on borate materials is difficult to measure because they have mechanical and crystal water and the temperature to heat samples to to remove only the former is difficult to assess.

Thus, the test is done this way:
-Take ten samples (from 10 bags) and mix well
-Weigh a bisque-fired bowl and dry and mark the weight on it
-Put powder straight from the bag into the bowl, weigh and mark
-Fire to cone 04
-Weight again and calculate the LOI

Variables

LOI - LOI (C)

This calculates the LOI as follows:
Bowl - B
Bowl+Powder - BP
Bowl Fired - BF

(BP-B) - (BF-B) / (BP-B) * 100

DWT - Dry Weight (V)

This is the weight of the powder. The powder should be from a sample that has been collected from at least 10 bags throughout the shipment.

FWT - Fired Weight (V)

The weight of the powder fired to cone 010.

Related Information

Links

Tests LOI (100-1000C)
Measure how much weight a dried clay test bar loses as it is fired in a kiln
Tests LOI/Density/Water Content
LDW LOI, density and water content test procedure for plastic clay bodies and porcelains
Typecodes Material Tests
Test conducted primarily on materials use to make bodies or glazes.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy