Pyrotrol 3503

Description: Andalusite/Pyrophyllite Ore

Oxide Analysis Formula Tolerance
K2O 0.20% 0.01
Na2O 0.20% 0.02
TiO2 0.40% 0.02
Al2O3 20.50% 1.00
SiO2 75.50% 6.25
Fe2O3 0.40% 0.01
LOI 2.80%n/a
Oxide Weight 483.63
Formula Weight 497.56

Notes

Chemically essentially the same as 2253, but finer: 100% -200 mesh and noted as 99% -325 mesh. Its bulk density is lower, 40 pcf instead of 45.

Related Information

Links

Materials Pyrotrol
URLs https://www.rescoproducts.com/docs/default-source/data-sheets-us/sds/pyrotrol-all-grades-msds.pdf?sfvrsn=905bb13b_5
SDS for all versions of Pyrotrol
URLs https://www.rescoproducts.com/docs/default-source/data-sheets-us/pds/pyrotrol-2253-and-2254-and-3503.pdf
Pyrotrol Data Sheet

Data

% Passing 325 Mesh Wet 99
Bulk Density lbs/cu. ft. (Packed) 40
Pyrometric Cone Equivalent 26

Mechanisms

Body Thermal ExpansionPyrotrol products impart higher strength in electrical porcelains and reduce dunting problems associated with traditional porcelain bodies if substituted for silica content.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy