1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Pemco Frit P-586

Alternate Names: Frit 586, Frit P586

Description: Barium, zinc, calcium frit for partially fritted cone 4-10 glazes

Oxide Analysis Formula Tolerance
BaO 4.10% 0.05
CaO 14.30% 0.48
K2O 4.00% 0.08
MgO 0.60% 0.03
Na2O 1.60% 0.05
ZnO 13.40% 0.31
B2O3 4.50% 0.12
Al2O3 8.20% 0.15
SiO2 49.30% 1.55
Oxide Weight 188.88
Formula Weight 188.88

Related Information

Links

Materials Fusion Frit FZ-22
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Ferro Frit 3276
Materials Hommel Frit 1030
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 7.30
Co-efficient of Linear Expansion 7.5 x 10-6 (50-450C)
Frit Melting Range (C) 1600-1860F
I.F.P. (celsius) 689C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy