Pemco Frit P-1V31

Alternate Names: 1V31,1V-31

Description: Semi-opaque high zinc fast fire frit

Oxide Analysis Formula Tolerance
BaO 3.90% 0.05
CaO 13.40% 0.48
K2O 3.10% 0.07
MgO 0.60% 0.03
Na2O 1.70% 0.06
ZnO 12.70% 0.31
ZrO2 4.00% 0.07
B2O3 4.30% 0.12
Al2O3 5.30% 0.10
SiO2 51.00% 1.71
Oxide Weight 201.80
Formula Weight 201.80

Notes

Developed for use as all-fritted glaze at 1900 - 2000F

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 7.00
Co-efficient of Linear Expansion 7.00 (50-450C)
Frit Softening Point 1650F
Frit Melting Range (C) 1550-1750F
Co-efficient of Linear Expansion 7.0x10-6 (50-450C)
I.F.P. (celsius) 685C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy