Pemco Frit P-1733

Alternate Names: Frit 1733, Frit P1733

Description: Soda-zinc-borosilicate leadless frit

Oxide Analysis Formula Tolerance
CaO 4.20% 0.18
Na2O 9.40% 0.36
ZnO 15.50% 0.46
B2O3 30.20% 1.04
SiO2 40.70% 1.62
Oxide Weight 239.87
Formula Weight 239.87

Notes

Good for reds and oranges, textured glaze applications.
Used in single-application textured glazes.

This is a very high zinc frit. It would be useful for cone 6 or lower crystalline glazes using a recipe of about 90 frit and 10 kaolin.

Related Information

Links

Materials General Frit GF-110
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Fusion Frit FZ-16
The champion in our frit melt-off competitition. This frit showcases the amazing fluxing power of boron and zinc working together. It is 15.5% ZnO.
Materials Hommel Frit 446
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 7.90 (50-450C)
Frit Melting Range (C) 1400-1500F
I.F.P. (celsius) 570C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy