M&D Ball Clay

Description: Missouri Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.50% 0.03
K2O 0.50% 0.02
MgO 0.50% 0.05
TiO2 1.31% 0.06
Al2O3 27.33% 1.00
SiO2 57.46% 3.57
Fe2O3 2.31% 0.05
LOI 10.09%n/a
Oxide Weight 335.56
Formula Weight 373.22

Notes

A very fine-grained montmorillontic bearing ball clay with exceptional strength and plasticity. M&D is considered the strongest ball clay on the market today. It is used primarily in plastic formed bodies, and by the refractories and electrical porcelain industries.

Physical Properties
===================
Water of Plasticity*: 37.0%
% Dry Shrinkage*: 6.5
Dry M.O.R., psi:* 825
pH: 4.4
C.E.C., meq/100g: 11.0
Specific Surface Area, sq metre/g: 24.4
Soluble sulfur+: Low

P.C.E.: 32

Particle Size, Microns: 20 10 5 2 1 0.5 0.2
(% finer than) 99% 97% 93% 81% 72% 56% 35%

Fired Properties
================
Cone 5 10
----
Total Shrinkage: 13.0% 14.5%
Absorption: 10.0% 1.0%

Shipped from Mayfield, KY

------------------
*Extruded, 50% ball clay, 50% flint
+Low-trace to 150, Med-150-400, High-450+
**50% Clay, 50% Nepheline Syenite

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy