Alternate Names: Kaolen 115
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.09% | 0.01 | |
| MgO | 0.29% | 0.03 | |
| K2O | 0.12% | - | |
| Na2O | 0.13% | 0.01 | |
| TiO2 | 0.43% | 0.02 | |
| Al2O3 | 28.17% | 1.00 | |
| SiO2 | 59.46% | 3.58 | |
| Fe2O3 | 0.51% | 0.01 | |
| LOI | 10.80% | n/a | |
| SO4 | 0.65% | n/a | |
| Oxide Weight | 322.98 | ||
| Formula Weight | 364.75 | ||
Available in run-of-mine, 25mm and 50mm sizes.
| Minerals |
Quartz
Quartz is the most abundant mineral on earth, it is the main crystalline mineral form of silica (SiO |
| Minerals |
Kaolinite
The most fundamental clay mineral. This mineral is found in nature in its purest form as kaolin. How |
| Typecodes |
Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content. |
| Materials |
Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries. |
| Materials |
Kaolin 143
|
| Materials |
Kaolin 114
|
| Materials |
Kaolin 113
|
| Materials |
Kaolin 111
|
| Materials |
Kaolin 171
|
| Materials |
Kaolin 151
|
| Firing Shrinkage | 1000C: 8.0% 1100C: 9% 1200C: 11% 1250C: 12.5% |
|---|---|
| Water absorption | 1000C: 17.5% 1100C: 17% 1200C: 14% 1250C: 12.5% |