1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

General Frit GF-9

Alternate Names: Frit 9, Frit GF9

Description: High Lead Zincless Glaze Frit

Oxide Analysis Formula Tolerance
K2O 1.54% 0.05
Na2O 0.40% 0.02
PbO 67.70% 0.93
Al2O3 2.33% 0.07
SiO2 28.03% 1.43
Oxide Weight 306.64
Formula Weight 306.64

Notes

Cone Range: 08-02
Very low melting temperature.

Related Information

Links

Materials Pemco Frit Pb-723
Materials Ferro Frit 3403
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Typecodes Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 7.20
Frit Softening Point 1350F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy