Description: Lead alumina bisilicate frit
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.10% | 0.01 | |
| K2O | 1.40% | 0.05 | |
| Na2O | 0.30% | 0.01 | |
| PbO | 67.80% | 0.93 | |
| Al2O3 | 2.30% | 0.07 | |
| SiO2 | 28.10% | 1.44 | |
| Oxide Weight | 307.46 | ||
| Formula Weight | 307.46 | ||
Cone Range: 08-02
This is basically a lead bisilicate frit with a few impurities.
Very low melting temperature.
| Materials |
Fusion Frit FL-42
|
| Materials |
Hommel Frit 437
|
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Materials |
Ferro Frit 3602
A lead bisilicate frit with 2.5% alumina oxide. |
| Materials |
General Frit GF-9
|
| Materials |
Pemco Frit Pb-723
|
| Materials |
Lead Bisilicate Frit
A standard frit of 1 molar part of PbO and 2 of SiO2. It is considered stable and non-leachable. |
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Typecodes |
Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out. |
| Co-efficient of Linear Expansion | 7.2 |
|---|---|
| Frit Melting Range (C) | 1350F |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk