General Frit GF-115

Alternate Names: Frit 115, Frit GF115

Description: High Calcium Boron Leadless for partially-fritted tile glazes

Oxide Analysis Formula Tolerance
CaO 11.43% 0.68
Na2O 5.95% 0.32
B2O3 23.15% 1.11
Al2O3 11.92% 0.39
SiO2 47.55% 2.64
Oxide Weight 333.65
Formula Weight 333.65

Related Information

Links

Materials Fusion Frit F-2
Materials F-2 Ball Clay
Materials Ferro Frit 3195
A commonly available calcium borosilicate frit. It is glaze-like, needing only a kaolin addition to create a low-temperature semi-glossy glaze.
Materials Pemco Frit P-67
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 6.90
Frit Softening Point 1800F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy