1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Fusion Frit FZ-24

Alternate Names: Frit FZ24

Description: High expansion leadless frit

Oxide Analysis Formula Tolerance
BaO 1.40% 0.02
CaO 3.00% 0.13
K2O 8.00% 0.21
Na2O 14.70% 0.58
ZnO 2.20% 0.07
B2O3 6.20% 0.22
Al2O3 10.00% 0.24
SiO2 54.50% 2.20
Oxide Weight 242.92
Formula Weight 242.92

Notes

This is used as an addition to low and medium fire glazes to increase their thermal expansion to solve shivering problems.

Related Information

Links

Materials Fusion Frit F-524
A low fire base glaze, add 10% kaolin, adjust thermal expansion using other frits.
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 11.13 x 10-6
Frit Softening Point 1450F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy