1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Fusion Frit FZ-14

Alternate Names: Fusion Frit FZ14

Description: Zinc low boron frit for cone 1 glazes

Oxide Analysis Formula Tolerance
CaO 6.50% 0.27
K2O 3.00% 0.07
Na2O 10.00% 0.37
ZnO 10.00% 0.28
B2O3 5.00% 0.17
Al2O3 14.00% 0.32
SiO2 51.50% 1.98
Oxide Weight 231.56
Formula Weight 231.56

Notes

This analysis was confirmed with Fusion Sept 2013.

Related Information

Links

Materials Pemco Frit P-991
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Hommel Frit 2GF27D
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 9.53 x 10-6
Frit Softening Point 1600F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy