Frit FA-233-2 (approx)

Alternate Names: Frit FA233-2

Description: Zircon opacified zinc borate frit for opaque glazes

Oxide Analysis Formula Tolerance
SiO2 47.50% 2.64 2.5
B2O3 17.50% 0.84 2.5
Na2O 2.50% 0.13 2.5
K2O 0.50% 0.02 .5
CaO 12.50% 0.74 2.5
Al2O3 7.50% 0.25 2.5
ZnO 2.50% 0.10 2.5
ZrO2 12.50% 0.34 2.5
Oxide Weight 344.30
Formula Weight 344.30

Notes

This is a USA pottery frit.
As of 2008 Ferro only published an approximate analysis, that is shown here.

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.
Typecodes Available from Laguna Clays
URLs https://digitalfire.com/4sight/datasheets/ferropotteryfrits2008.pdf
Ferro Pottery Frits 2008

Data

Co-efficient of Linear Expansion 7.04
Frit Softening Point 1650F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy