1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Ferro Frit 3300

Alternate Names: F3300

Description: Medium lead high zinc glaze for for cone 02-8

Oxide Analysis Formula Tolerance
BaO 6.20% 0.08
CaO 8.80% 0.33
K2O 3.20% 0.07
MgO 0.40% 0.02
Na2O 0.70% 0.02
PbO 22.20% 0.21
ZnO 10.50% 0.27
Al2O3 9.20% 0.19
SiO2 38.80% 1.34
Oxide Weight 207.92
Formula Weight 207.92

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Fusion Frit FZ-35
Materials Hommel Frit 316
Materials Fusion Frit FZ-45
Typecodes Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 8.30
Co-efficient of Linear Expansion 8.30 x 10-6
Frit Softening Point 1700F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy