Oxide Analysis Formula Tolerance
CaO 0.30% 0.02
K2O 2.34% 0.09
MgO 0.33% 0.03
Na2O 0.22% 0.01
Fe2O3 2.28% 0.05
Al2O3 28.08% 1.00
SiO2 55.83% 3.37
TiO2 0.60% 0.03
SO4 0.53%n/a
C 0.23%n/a
LOI 10.02%n/a
Organics 0.40%n/a
Oxide Weight 326.85
Formula Weight 367.99

Related Information

Links

Minerals Quartz
Quartz is the most abundant mineral on earth, it is the main crystalline mineral form of silica (SiO
Minerals Kaolinite
The most fundamental clay mineral. This mineral is found in nature in its purest form as kaolin. How
Minerals Na-Feldspar
Most common feldspars contain both sodium and potassium. The term Na-Feldspar designates one where t
Minerals K-Feldspar
Most common feldspars contain both sodium and potassium. The term K-Feldspar designates one where th
Minerals Organics
Ceramic minerals can contain lignite, fibrous plant material, etc. These burn out on firing.
Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.
Materials Clay 220
Materials Clay 244
Materials Clay 233
Materials Clay 232
Materials Clay 261
Materials Clay 246
Materials Clay 220
Materials Clay 216
Materials Clay 215

Data

Dry Strength (kgf/cm2) 45.0
Firing Shrinkage 1050C: 2.0% 1100C: 5.0% 1150C: 9.0% 1200C: 12.0% 1250C: 14.0%
Sieve Analysis Dry < 212 micron: 98.9% < 150 micron: 98.0% < 106 micron: 97.1% < 63 micron: 94.7% < 45 micron: 93.
Water absorption 1050C: 20.0% 1100C: 16.5% 1150C: 8.0% 1200C: 5.0% 1250C: 3.0%

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy