Alternate Names: Frit B-300
Description: Lead alumina bilsilicate frit
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| PbO | 65.00% | 1.00 | |
| Al2O3 | 3.00% | 0.10 | |
| SiO2 | 32.00% | 1.83 | |
| Oxide Weight | 343.38 | ||
| Formula Weight | 343.38 | ||
Raw color: Very light yellow
Form: Granular or finely ground frit
Specific Gravity: 4.6 g/cm3
Density, lbs/cu ft, Granlar: 155-175; Ground: 135-155
Melting Range: 788-816C
COE: 7.1 x 10-6
The powdered material is ~2% +200 mesh.
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Materials |
Frit 3647
|
| Materials |
Ceraflux
|
| Materials |
Ferro Frit 3489
|
| Materials |
BPS Lead Bisilicate
|
| Materials |
Lead Bisilcate B-15
|
| Materials |
Lead Bisilicate Frit
A standard frit of 1 molar part of PbO and 2 of SiO2. It is considered stable and non-leachable. |
| Materials |
Ferro Frit 3626
|
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Typecodes |
Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out. |
| URLs |
https://hammondglobal.com/wp-content/uploads/2022/06/Ceraflux-0512.pdf
Hammond Lead Products Ceraflux lead bisilicate data sheet Specially formulated for use in pottery and wall-tile glazes. Lead bisilicate is extremely resistant to leaching by dilute acids, including gastric juices, which reduces its toxicity and offers the maximum safety of any of the lead products. Available in either granulated or ground form. |
| Frit Softening Point | 800C |
|---|---|
| Frit Softening Point | 788-816C |
| Density (Specific Gravity) | 4.50 |
| Density (Specific Gravity) | 4.55-4.7 |