APG Missouri Fireclay

Alternate Names: AP Green, A.P., A. P., APG Fire, APGFC

Description: Buff Burning Plastic Fireclay

Oxide Analysis Formula Tolerance
CaO 0.35% 0.02
K2O 0.50% 0.02
MgO 0.35% 0.03
Na2O 0.50% 0.03
TiO2 2.00% 0.08
Al2O3 31.00% 1.00
SiO2 52.00% 2.85
Fe2O3 2.00% 0.04
LOI 11.00%n/a
Oxide Weight 291.85
Formula Weight 327.92

Notes

A popular medium plasticity buff burning clay used in stoneware, sculpture and many other types of clay bodies. It is very refractory (8-10% absorption, 12% total shrinkage cone 10) and fires to an attractive surface. It is considered very consistent.

It is also used for mortar for building kilns.

20 mesh grade:
0-0.5% on 14 mesh
0.5-10.0 on 20 mesh
35.0-50.0 through 100 mesh

28 mesh grade:
0.5-5.0 on 20 mesh
0.5-10.0 on 28 mesh
20.0-38.0 through 100 mesh

PCE; 30-31.5

Related Information

Links

Articles Duplicating AP Green Fireclay
Few people actually understood what AP Green fireclay really was (it is no longer available). By carefully ascertaining its physical properties we were able to formulate a substitute material mix.
Typecodes Fireclay
Fireclays are non-kaolin non-ball clay materials similar to stoneware clays but lacking fluxing oxides. Many fireclays have a PCE of 28 or more.
Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.
Materials Fireclay
Materials Imco 400 Fireclay
Materials Plainsman Fireclay
Materials Pine Lake Fireclay
Materials Hawthorn Bond
Materials NAT Dry Milled Fireclay
URLs https://www.asbestos.com/companies/a-p-green-industries.php
AP Green Asbestos Use

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy