Kaosand

Description: Plainsman Native Clay

Oxide Analysis Formula Tolerance
BaO 0.32% 0.01
CaO 0.22% 0.02
K2O 2.32% 0.15
MgO 0.56% 0.08
Na2O 0.14% 0.01
TiO2 0.65% 0.05
Al2O3 17.20% 1.00
P2O5 0.15% 0.01
SiO2 70.43% 6.95
Fe2O3 1.30% 0.05
MnO 0.01% -
LOI 6.70%n/a
Oxide Weight 553.29
Formula Weight 593.02

Notes

A fine white firing, kaolinized sand, suitable as a body constituent to diversify particle size, add texture, improve drying and reduce plasticity. This material has very low plasticity and cannot be used by itself. It is a very unique material, not available anywhere else that we know of.

Sieve Analysis Wet Washed
(Root of 2 series) +35 +48 +65 +100 +150# +200 +325
---------------------------------------------
0.2% 0.5% 7.6% 22.9% 30.9% 38.2% n/a

Texture: Sandy
Plastic Index (1-10): 1
Green Strength (lbs/sqaure inch): n/a
Dry shrinkage: n/a
Dried density: 1.85
PCE: 20.5

Related Information

Links

Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.

Data

Frit Softening Point PCE 21

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy