PotteryCrafts Frit P2953

Alternate Names: PotteryCrafts Frit 2953

Description: Borax frit

Oxide Analysis Formula Tolerance
CaO 14.10% 0.61
K2O 1.70% 0.04
MgO 0.10% 0.01
Na2O 8.80% 0.34
B2O3 18.00% 0.62
Al2O3 7.50% 0.18
SiO2 49.60% 1.99
LOI 0.20%n/a
Oxide Weight 241.18
Formula Weight 241.66

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Potclays Frit 2265
Materials BPS Standard Borax Frit
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.
URLs http://www.potterycrafts.co.uk/Products/0028000b
PotteryCrafts Frit information

Data

Co-efficient of Linear Expansion 8.3
Frit Melting Range (C) 900-1100C