Error: API server returned an invalid response for materialAlternate Names: Fusion Frit F95
Description: Opacified flux for wall tile
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| BaO | 0.50% | 0.01 | |
| CaO | 4.00% | 0.28 | |
| K2O | 2.50% | 0.10 | |
| Na2O | 9.50% | 0.60 | |
| ZrO2 | 17.20% | 0.55 | |
| B2O3 | 17.50% | 0.99 | |
| Al2O3 | 7.00% | 0.27 | |
| SiO2 | 41.50% | 2.72 | |
| Oxide Weight | 392.01 | ||
| Formula Weight | 392.01 | ||
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Materials |
Frit 282-b
|
| Materials |
Hommel Frit 477
|
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Co-efficient of Linear Expansion | 7.35 x 10-6 |
|---|---|
| Frit Softening Point | 1500F |