Fusion Frit F-5

Alternate Names: Fusion Frit F5

Description: Strontium Barium flux

Oxide Analysis Formula Tolerance
CaO 10.22% 0.49
BaO 11.73% 0.21
Na2O 1.72% 0.07
K2O 2.42% 0.07
SrO 6.04% 0.16
Al2O3 5.14% 0.14
B2O3 6.12% 0.24
SiO2 56.62% 2.54
Oxide Weight 269.99
Formula Weight 269.99

Related Information

Links

URLs http://www.fusionceramics.com/
Fusion Ceramics Frit Website
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 7.13 x 10-6
Frit Softening Point 1800F