Wilco-UPF Kaolin

Oxide Analysis Formula Tolerance
SiO2 45.80% 2.06
Fe2O3 0.70% 0.01
Al2O3 37.70% 1.00
TiO2 1.70% 0.06
CaO 0.10% -
LOI 13.20%n/a
Oxide Weight 232.68
Formula Weight 268.06

Notes

Wilco UPF is finer grained kaolin and can be employed in a ceramic formulation where higher permeability type kaolin is not required. It has excellent suspension qualities and lends good film strength to ceramic engobes and glazes of all temperature ranges. Wilco UPF also meets the requirements of filler applications where a dry ground processed kaolin can be employed.

This is not suitable for use in making plastic bodies that depend primarily on it for the plasticity. Thus it cannot be used in recipes as a substitute for #6 Tile kaolin, for example.

Related Information

Links

Typecodes Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content.
Materials Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries.
Materials Pioneer Kaolin
URLs http://www.oldhickoryclay.com/wilco-upf.html
Old Hickory Wilco-UPF Data Sheet

Data

Pyrometric Cone Equivalent 34

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy