Whitemud Kaolin

Description: Airfloated sedimentary kaolin

Oxide Analysis Formula Tolerance
Al2O3 30.50% 1.00 1.5
SiO2 54.00% 3.00 2
Fe2O3 1.50% 0.03
TiO2 0.80% 0.03
CaO 0.30% 0.02
MgO 0.13% 0.01
Na2O 0.04% -
K2O 1.15% 0.04
LOI 11.50%n/a
Oxide Weight 295.70
Formula Weight 334.12

Notes

A high-quality, air floated, sedimentary kaolin clay separated from the kaolinized sands of southern Saskatchewan, Canada.

Related Information

Links

Typecodes Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content.
Materials Whitemud Meta Kaolin

Data

GE Brightness 66-69
Density, loose packed (lbs/cu fut) 30-35
Density (Specific Gravity) 2.6
Median Particle Size (Microns) 3-7 microns
% < 30 microns 90%

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy