MC Na-200 Feldspar

Alternate Names: NA200, MC NA 200

Oxide Analysis Formula Tolerance
SiO2 64.84% 5.55
Al2O3 20.71% 1.04
Fe2O3 0.06% -
CaO 1.82% 0.17
Na2O 6.49% 0.54
K2O 5.20% 0.28
BaO 0.33% 0.01
LOI 0.40%n/a
Oxide Weight 511.38
Formula Weight 513.43

Notes

The company was introducing this January 2007 and claimed: "A high quality sodium/potassium/calcium aluminum silicate, ground to 200 mesh for ceramic applications. Carefully beneficiated and controlled for quality, it offers a high alkali content and low iron oxide content per unit of alumina."
Cone 11 fired flow tests beside MC K-325 show this to melt much better even though it is a larger particle size. It also melts much better than Custer or G-200 and the melt flow is whiter than G-200 and much whiter than Custer.

Related Information

Feldspars, the primary high temperature flux, melt less than you think.


Feldspar melt flows at cone 8 and 11

This picture has its own page with more detail, click here to see it.

Our melt fluidity tester is being used to compare cone 8 melt fluidities of Custer, G-200 and i-Minerals high soda and high potassium feldspars. Notice how little the pure materials are moving (bottom), even though they are fired to cone 11. In addition, the sodium feldspars move better than the potassium ones. But feldspars do their real fluxing work when they can interact with other materials. As a demonstration of that, note how well they flow with only 10% frit added (top), even though fired three cones lower.

Links

Materials Potash Feldspar
A feldspar having a KNaO content that predominates in potassium.
Materials Soda Feldspar
A feldspar having a KNaO content that predominates in sodium.
Typecodes Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies.

Data

Bulk Density lbs/cu. ft. (Packed) 90
Sieve Analysis Dry +140 mesh: 0.5 max +200: 1.5 max +325: 10.0 max